Sterilization ceramic plate and preparation method thereof
A technology of ceramic plates and cordierite, applied in the field of sterilized ceramic plates and their preparation, can solve problems such as unfavorable healthy growth of pets, hidden dangers to human health and safety, water accumulation in pet utensils, etc., and achieves easy processing and promotion, good sterilization effect,  Long service life effect
- Summary
 - Abstract
 - Description
 - Claims
 - Application Information
 
 AI Technical Summary 
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] A sterilized ceramic plate, the raw material composition of the sterilized ceramic plate includes cordierite, mullite, high alumina, binder, copper sulfate, titanium oxide, water, and is weighed according to the mass percentage of the following components:
[0027] Cordierite 10%;
[0028] Mullite 30%;
[0029] High aluminum 18%;
[0030] Binder 5%;
[0031] Copper sulfate 0.2%;
[0032] Titanium oxide 0.4%.
[0033] The preparation method of the sterilized ceramic plate of the present embodiment comprises the steps:
[0034] S1: Spray and dry cordierite, mullite, high alumina, binder, copper sulfate, and titanium oxide respectively, then carry out particle crushing, then filter, remove iron, and set aside;
[0035] S2: Add water to the raw materials in S1, stir and mix, stale for 36-64 hours, and set aside;
[0036] S3: The mixed material in S2 is pressed and formed, light pressure exhausted, heavy pressure exhausted, heavy pressure formed, and then prepared into...
Embodiment 2
[0043] A sterilized ceramic plate, the raw material composition of the sterilized ceramic plate includes cordierite, mullite, high alumina, binder, copper sulfate, titanium oxide, water, and is weighed according to the mass percentage of the following components:
[0044] Cordierite 12%;
[0045] Mullite 38%;
[0046] High aluminum 25%;
[0047] Binder 8%;
[0048] Copper sulfate 0.4%;
[0049] Titanium oxide 0.6%.
[0050] The preparation method of the sterilized ceramic plate of the present embodiment comprises the steps:
[0051] S1: Spray and dry cordierite, mullite, high alumina, binder, copper sulfate, and titanium oxide respectively, then carry out particle crushing, then filter, remove iron, and set aside;
[0052] S2: Add water to the raw materials in S1, stir and mix, stale for 48 hours, and set aside;
[0053] S3: The mixed material in S2 is pressed and formed, light pressure exhausted, heavy pressure exhausted, heavy pressure formed, and then prepared into a ...
Embodiment 3
[0060] A sterilized ceramic plate, the raw material composition of the sterilized ceramic plate includes cordierite, mullite, high alumina, binder, copper sulfate, titanium oxide, water, and is weighed according to the mass percentage of the following components:
[0061] Cordierite 15%;
[0062] Mullite 45%;
[0063] High aluminum 35%;
[0064] Binder 10%;
[0065] Copper sulfate 0.6%;
[0066] Titanium oxide 1%.
[0067] The preparation method of the sterilized ceramic plate of the present embodiment comprises the steps:
[0068] S1: Spray and dry cordierite, mullite, high alumina, binder, copper sulfate, and titanium oxide respectively, then carry out particle crushing, then filter, remove iron, and set aside;
[0069] S2: Add water to the raw materials in S1, stir and mix, stale for 64 hours, and set aside;
[0070]S3: The mixed material in S2 is pressed and formed, light pressure exhausted, heavy pressure exhausted, heavy pressure formed, and then prepared into a ce...
PUM
 Login to View More Abstract
Description
Claims
Application Information
 Login to View More - R&D
 - Intellectual Property
 - Life Sciences
 - Materials
 - Tech Scout
 
- Unparalleled Data Quality
 - Higher Quality Content
 - 60% Fewer Hallucinations
 
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com