Production method for improving creped paper for taste-absorbing cigarette holder
A production method and technology for creping paper, applied in the field of papermaking, to achieve the effects of improving suction experience, improving softness and excellent taste
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0085] Example 1: Hybrid coating
[0086] 1. Main raw materials:
[0087] Wet strength agent: PAE, the mass percentage concentration is 0.5-1.5%;
[0088] Flavors and fragrances: the mass percentage concentration is 1.5-15%;
[0089] Glycerin: the mass percentage concentration is 1-5%;
[0090] Mixed coating solution: mix the flavor and fragrance with glycerin to prepare a mixed coating solution, the weight ratio of the flavor and fragrance to glycerin is 90-98% and 2-10% respectively.
[0091] 2. Main equipment:
[0092] Five-color printing presses, paint preparation tanks.
[0093] 3. Method steps:
[0094] (1) Creping base paper roll
[0095] The base paper rolls of crepe paper are produced by the wet process.
[0096] When making crepe base paper rolls, wet strength agent PAE is added to the pulp, and the wet strength is 0.1-0.5 kN / m.
[0097] (2) Coating: mixed coating process
[0098] A printing machine is used to coat the mixed coating solution on the crepe pap...
Embodiment 2
[0107] Example 2: Separate coating
[0108] 1. Main raw materials:
[0109] Wet strength agent: PAE, the mass percentage concentration is 0.5-1.5%;
[0110] Flavors and fragrances: the mass percentage concentration is 1.5-15%;
[0111] Glycerin: the mass percent concentration is 1-5%.
[0112] 2. Main equipment:
[0113] Five-color printing presses, paint preparation tanks.
[0114] 3. Method steps:
[0115] (1) Creping base paper roll
[0116] The base paper roll of creping paper made by wet papermaking process.
[0117] When making crepe base paper rolls, wet strength agent PAE is added to the pulp, and the wet strength is 0.1-0.5 kN / m.
[0118] (2) Coating: mixed coating process
[0119] Use a printing machine to first coat glycerin on the crepe paper, the coating amount is 0.1-1%, and then apply flavor and fragrance, the coating amount is 0.5-10%.
[0120] When coating, the vehicle speed is 15-80m / min.
[0121] (3) drying
[0122] After coating, dry in an oven w...
Embodiment 3
[0128] Embodiment 3: mixed coating
[0129] 1. Main raw materials:
[0130] Wet strength agent: PAE, the mass percentage concentration is 0.5-1.5%;
[0131] Flavors and fragrances: the mass percentage concentration is 1.5-15%;
[0132] Propylene glycol: the mass percentage concentration is 1-5%;
[0133] Mixed coating solution: mix the flavor and fragrance with propylene glycol to prepare a mixed coating solution, the weight ratio of the flavor and fragrance to glycerin is 90-98% and 2-10% respectively.
[0134] 2. Main equipment:
[0135] Five-color printing presses, paint preparation tanks.
[0136] 3. Method steps:
[0137] (1) Creping base paper roll
[0138] The base paper roll of creping paper made by wet papermaking process.
[0139] When making crepe base paper rolls, wet strength agent PAE is added to the pulp, and the wet strength is 0.1-0.5 kN / m.
[0140] (2) Coating: mixed coating process
[0141] A printing machine is used to coat the mixed coating solution...