A treatment method and wood veneer technology, which is applied in the field of primer treatment of wood veneer panels, can solve the problems of furniture panels containing paint smell, increasing the cost of panel manufacturing, consuming large paint and manpower, etc., achieving short hot pressing time, Ensure product quality and reduce scratches
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0038] Step 1. Glue adjustment
[0039] Put the protein glue into the container, add soybean powder, the mass ratio of protein glue and soybean powder is 10:5, stir well to make it sticky and free of particles;
[0040] Step two, glue
[0041] Pour the prepared glue into the glue applicator and adjust the amount of glue to 200g / m 2 , apply glue on the ash density board, the plain board before the glue is as figure 1 As shown, the board after gluing is as follows figure 2 As shown, the smear is even and the penetration effect is good;
[0042] Step three, glue
[0043] The press is preheated, the pressure is 12mpa, the temperature is 120°C, and the hot pressing time is 70 seconds, so that the glue can fully fill the cell pores of the wood veneer. Under the action of temperature and pressure, the soybean protein glue can fully fill the cell pores and then solidify instantly;
[0044] Step 4: Spray topcoat, the effect is as follows image 3 As shown, the paint surface is a...
Embodiment 2
[0046] Step 1. Glue adjustment
[0047] Put the protein glue into the container, add soybean powder, the mass ratio of protein glue and soybean powder is 10:3, stir well to make it sticky and free of particles;
[0048] Step two, glue
[0049] Pour the prepared glue into the glue applicator, and adjust the amount of glue to 180g / m 2 , glued on birch chipboard;
[0050] Step three, glue
[0051] The press is preheated, the pressure is 15mpa, the temperature is 120°C, and the hot pressing time is 75 seconds, so that the glue can fully fill the cell pores of the wood veneer. Under the action of temperature and pressure, the soybean protein glue fully fills the cell pores and then solidifies instantly;
[0052] Step 4, spray finish paint, effect is the same as embodiment 1.
Embodiment 3
[0054] Step 1. Glue adjustment
[0055] Put the protein glue into the container, add soybean powder, the mass ratio of protein glue and soybean powder is 10:1, stir well to make it sticky and free of particles;
[0056] Step two, glue
[0057] Pour the prepared glue into the glue applicator, and adjust the amount of glue to 150g / m 2 , apply glue on the rubber wood OSB board;
[0058] Step three, glue
[0059]The press is preheated, the pressure is 15mpa, the temperature is 110°C, and the hot pressing time is 80 seconds, so that the glue can fully fill the cell pores of the wood veneer. Under the action of temperature and pressure, the soybean protein glue can fully fill the cell pores and then solidify instantly;
[0060] Step 4, spray finish paint, effect is the same as embodiment 1.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com