Asphalt aging repairing agent and preparation and use methods thereof
A repairing agent and asphalt technology, applied in building components, building insulation materials, construction and other directions, can solve the problems of large construction investment, poor economic and social benefits, time-consuming and labor-intensive in regeneration treatment technology, and achieve resistance to ultraviolet light aging, The effect of improving penetration and diffusion ability and strong wear resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0025] The invention also provides a preparation method of the asphalt aging repair agent, which includes the following steps:
[0026] Step 1. Dissolve phthalate, polyoxyethylene ether compound and sulfolane in water to obtain a continuous phase mixed solution, and the continuous phase mixed solution is used as a material for standby;
[0027] Add rubber oil and polyvinyl alcohol to the emulsified asphalt, stir for 5-10min at room temperature, at a stirring rate of 200-400rad / min, to obtain a continuous phase emulsion, add hindered amine stabilizer and nano-titanium dioxide, and slowly stir until particles Dissolve, slowly stirring rate is 200 ~ 400rad / min, stirring time is 5-10min; then at a heating rate of 5-6 ℃, heating up to 60-70 ℃, continue to stir slowly until a stable solution is formed, slowly stirring time is 200 ~ 400rad / min, stirring time is 10-15min; cooling to room temperature, get material 2 for use;
[0028] Step 2. Put the above-mentioned material 1 and material 2 ...
Embodiment 1
[0033] An asphalt aging repair agent, in parts by mass, including rubber oil: 25 parts, emulsified asphalt: 21 parts, phthalate: 12 parts, polyoxyethylene ether compound: 4 parts, polyvinyl alcohol: 5 parts , Sulfolane: 10 parts, ultra-fine cement: 5 parts, light stabilizer 770: 3 parts, nano-titanium dioxide: 3 parts, water: 12 parts.
[0034] Among them, the emulsified asphalt uses ordinary emulsified asphalt, and the solid content of ordinary emulsified asphalt is 35%; the ultra-fine cement is P.O42.5 type ultra-fine cement with a specific surface area greater than 1000m 2 / kg, the average particle size is less than 8μm; the fineness of the light stabilizer 770 is 500nm, and the fineness of nano-titania is 40nm; tap water is used for water.
[0035] The preparation method of an asphalt aging repair agent described in Example 1, includes the following steps:
[0036] Step 1. Dissolve phthalate, polyoxyethylene ether compound and sulfolane in water to obtain a continuous phase mixed...
Embodiment 2
[0040] An asphalt aging repair agent, in parts by mass, including rubber oil: 30 parts, emulsified asphalt: 22, phthalate: 10 parts, polyoxyethylene ether compound: 3 parts, polyvinyl alcohol: 7 parts, Sulfolane: 8 parts, ultrafine cement: 7 parts, light stabilizer 770: 3 parts, nano titanium dioxide: 2 parts and water: 8 parts.
[0041] Among them, the emulsified asphalt uses ordinary emulsified asphalt, and the solid content of ordinary emulsified asphalt is 40%; the ultra-fine cement is P.O42.5 type ultra-fine cement with a specific surface area greater than 1000m 2 / kg, the average particle size is less than 8μm; hindered amine stabilizer uses light stabilizer 770, the fineness of light stabilizer 770 is 400nm; nanometer titanium dioxide fineness is 30nm; water uses tap water.
[0042] The preparation method of an asphalt aging repair agent described in Example 2 includes the following steps:
[0043] Step 1. Dissolve phthalate, polyoxyethylene ether compound and sulfolane in wat...
PUM
| Property | Measurement | Unit |
|---|---|---|
| Specific surface area | aaaaa | aaaaa |
| Particle size | aaaaa | aaaaa |
Abstract