Mimic enzyme catalyst preparation method and application thereof
An enzyme catalyst and catalyst technology, applied in the field of nanomaterials, can solve the problems of easy burying of edge active sites, unfavorable biological application research, complicated preparation methods, etc., and achieve the effects of shortening preparation time, excellent bacterial killing effect, and improving antibacterial performance.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0018] (1) Dissolve 260 mg of ammonium tetrathiomolybdate in 15 mL of dimethylformamide to obtain a dispersion, then add 1 mL of 1 mg / mL graphene oxide solution into the dispersion, and stir evenly;
[0019] (2) Add the above-mentioned dispersion into the reactor, and heat it to 200°C for 10 hours under stirring using a microwave reactor;
[0020] (3) Filter the solution after the reaction in step (2), wash the generated precipitate with deionized water and ethanol, and then dry the separated precipitate. That is, a molybdenum disulfide / graphene composite catalyst with high-efficiency enzyme-like catalytic activity is obtained.
Embodiment 2
[0034] (1) Dissolve 260 mg of ammonium tetrathiomolybdate in 15 mL of dimethylformamide to obtain a dispersion, then add 0.5 mL of 1 mg / mL graphene oxide solution into the dispersion, and stir evenly;
[0035] (2) Add the above dispersion liquid into the reactor, and heat it to 190°C for 6 hours under the condition of stirring by microwave reactor;
[0036] (3) Filter the solution after the reaction in step (2), wash the generated precipitate with deionized water and ethanol, and then dry the separated precipitate. That is, a molybdenum disulfide / graphene composite catalyst with high-efficiency enzyme-like catalytic activity is obtained.
Embodiment 3
[0038] (1) Dissolve 260 mg of ammonium tetrathiomolybdate in 15 mL of dimethylformamide to obtain a dispersion, then add 5 mL of 1 mg / mL graphene oxide solution into the dispersion, and stir evenly;
[0039] (2) Add the above-mentioned dispersion into the reactor, and heat it to 200°C for 10 hours under stirring using a microwave reactor;
[0040] (3) Filter the solution after the reaction in step (2), wash the generated precipitate with deionized water and ethanol, and then dry the separated precipitate. That is, a molybdenum disulfide / graphene composite catalyst with high-efficiency enzyme-like catalytic activity is obtained.
PUM
| Property | Measurement | Unit |
|---|---|---|