Process for accelerating wood ageing
A technology to accelerate aging and wood, applied in wood processing appliances, wood treatment, impregnated wood, etc., can solve problems such as loss of strength and use value
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] A wood accelerated aging process is carried out through the following steps in sequence:
[0017] 1. Use a flame spray gun to carbonize the wood surface: turn on the flame spray gun, and repeatedly bake the wood surface at a speed of 100mm / s along the direction of the wood grain until the wood surface is carbonized and blackened;
[0018] 2. Use a wire brush to gently brush off the carbonization on the wood surface: Use a wire brush to scrape the carbonized wood surface repeatedly until no carbonization falls off on the surface;
[0019] 3. Spray or brush evenly on the treated wood surface with 20% hydrogen peroxide, then dry until the moisture content is 15-30%, then spray or brush evenly on the treated wood surface with 20% hydrogen peroxide, and repeat the uniform spraying with 20% hydrogen peroxide Or brush on the treated wood surface, dry for 3 cycles, finally wash with water, dry, and dry the last time until the moisture content is 8-12%;
[0020] 4. Treat th...
Embodiment 2
[0022] A wood accelerated aging process is carried out through the following steps in sequence:
[0023] 1. Carbonize the wood surface with a flame spray gun: turn on the flame spray gun, and bake the wood surface repeatedly at a speed of 20mm / s along the direction of the wood grain until the wood surface is carbonized and blackened;
[0024] 2. Use a wire brush to gently brush off the carbonization on the wood surface: Use a wire brush to scrape the carbonized wood surface repeatedly until no carbonization falls off on the surface;
[0025] 3. Spray or brush evenly on the treated wood surface with 30% hypochlorous acid, then dry it to a moisture content of 15-30%, then spray or brush evenly on the treated wood surface with 30% hypochlorous acid, and finally use water Wash and dry until the moisture content is 8-12%;
[0026] 4. Treat the treated wood with a conventional finish.
Embodiment 3
[0028] A wood accelerated aging process is carried out through the following steps in sequence:
[0029] 1. Carbonize the wood surface with a flame spray gun: turn on the flame spray gun, and bake the wood surface repeatedly at a speed of 50mm / s along the wood grain direction until the wood surface appears carbonized and blackened;
[0030] 2. Use a wire brush to gently brush off the carbonization on the wood surface: Use a wire brush to scrape the carbonized wood surface repeatedly until no carbonization falls off on the surface;
[0031] 3. Spray or brush evenly on the treated wood surface with 10% sodium hypochlorite, then dry until the moisture content is 15-30%, and then spray or brush evenly on the treated wood surface with 10% sodium hypochlorite, repeat spraying 10% Sodium hypochlorite, air-dried or dried for 4 cycles, finally washed with water, dried, and dried for the last time to a moisture content of 8-12%;
[0032] 4. Treat the treated wood with a conventiona...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com