Modified nano SiO2 water quality processor turbidity standard substance and preparation method thereof
A water quality processor and turbidity technology, which is used in the field of standard material preparation to achieve good dilution characteristics, reduce force, and prevent agglomeration.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0041] Weigh 2g nano-SiO2 Dissolve in 60mL absolute ethanol, ultrasonically oscillate for 60min and then magnetically stir for 1h. 4.324g 3-chloropropyltrimethoxysilane was added to the dispersed nano-SiO 2 In the ethanol solution, react in a constant temperature water bath at 85°C for 0.5 h, then add 2 mL of 3 % volume concentration of hydrochloric acid, continue to react for 3.5 h, stir continuously during the reaction, after the reaction, centrifuge for 15 min, wash with absolute ethanol for 3 Second-rate. Dry in a vacuum oven at 55 °C for 8 h, grind into powder, and weigh an appropriate amount of modified nano-SiO 2 Powder, add tertiary water, ultrasonically disperse for 1 h, and prepare a spiked stock solution with a certain turbidity of about 400 NTU.
PUM
| Property | Measurement | Unit |
|---|---|---|
| The average particle size | aaaaa | aaaaa |
| The average particle size | aaaaa | aaaaa |
| The average particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com