A kind of thermal insulation wadding with air lock function and preparation method thereof
An air lock and flake technology, which is applied in hollow filament manufacturing, rayon manufacturing, physical treatment, etc., can solve the problems of poor air permeability, reducing the air permeability of clothes, and discharging to the outside environment.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] Immerse the three-dimensional crimped hollow polyester fiber in a mixed solution of ethanol and water with a weight ratio of 1, then add 3wt% zinc chloride to the mixed solution, heat it to 40°C, keep it warm for 2 hours, take it out, dry it, and obtain the modified Three-dimensional crimped hollow polyester fiber.
[0024] Mix viscose fiber, ES fiber and three-dimensional crimped hollow polyester fiber evenly to obtain fiber raw material; then open the fiber raw material twice and send it to a carding machine for carding to form fiber web fibers; then rearrange the fiber web fibers with random sticks , so that the fibers of the fiber web form a criss-cross structure; then, the treated fiber web fibers are sent to a layering machine for layering, and heated to 170° C., then cooled to obtain fiber flakes. Then, the fiber flakes are pre-punched and needled, and the surface of the fiber web fibers is sprayed with hydrogen peroxide at a concentration of 36wt% during the nee...
Embodiment 2
[0026] Immerse the three-dimensional crimped hollow polyester fiber in a mixed solution of ethanol and water with a weight ratio of 1, then add 5wt% zinc chloride to the mixed solution, heat it to 45°C, keep it warm for 2.5 hours, take it out, dry it, and obtain the modified Three-dimensional crimped hollow polyester fiber.
[0027] Mix viscose fiber, ES fiber and three-dimensional crimped hollow polyester fiber evenly to obtain fiber raw material; then open the fiber raw material twice and send it to a carding machine for carding to form fiber web fibers; then rearrange the fiber web fibers with random sticks , so that the fibers of the fiber web form a criss-cross structure; then, the treated fiber web fibers are sent to a layering machine for layering, heated to 175° C., and cooled to obtain fiber flakes. Then, the fiber flakes are pre-punched and needled, and the surface of the fiber web fibers is sprayed with hydrogen peroxide at a concentration of 36wt% during the needle...
PUM
Property | Measurement | Unit |
---|---|---|
length | aaaaa | aaaaa |
length | aaaaa | aaaaa |
length | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information

- R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com