Structure for curtain wall installation part and manufacturing material thereof
A technology for mounting structure and mounting parts, applied in the direction of walls, building components, building structures, etc., can solve the problems of easy cracking in the fixed position of the horizontal frame, structural corrosion of metal mounting parts, and reduced work efficiency, so as to overcome the rusting of metal. Fracture, simple installation mechanism, the effect of preventing the curtain wall from falling
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0037] A material for curtain wall installation parts, including the following components in mass percentage:
[0038] POM 92.5wt%;
[0039] 4-hydroxystyrene modified nitrile rubber 3.5wt%;
[0040] Anti-ultraviolet agent 1.5wt%;
[0041] Antioxidant 0.5wt%;
[0042] Compatibilizer 2wt%;
[0043] All the components were blended in proportion and then added to an extruder to extrude the material to obtain the material. The nozzle temperature of the extruder was 220°C, and the barrel temperature was 190°C.
Embodiment 2
[0045] A material for curtain wall installation parts, including the following components in mass percentage:
[0046] POM 90wt%;
[0047] 4-hydroxystyrene modified nitrile rubber 5wt%;
[0048] Anti-ultraviolet agent 1.5wt%;
[0049] Antioxidant 0.5wt%;
[0050] Compatibilizer 3wt%;
[0051] All the components were blended in proportion and then added to an extruder to extrude the material to obtain the material. The nozzle temperature of the extruder was 220°C, and the barrel temperature was 190°C.
Embodiment 3
[0053] A material for curtain wall installation parts, including the following components in mass percentage:
[0054] POM 95wt%;
[0055] 4-hydroxystyrene modified nitrile rubber 2wt%;
[0056] Anti-ultraviolet agent 0.5wt%;
[0057] Antioxidant 0.5wt%;
[0058] Compatibilizer 2wt%;
[0059] All the components were blended in proportion and then added to an extruder to extrude the material to obtain the material. The nozzle temperature of the extruder was 220°C, and the barrel temperature was 190°C.
PUM
Property | Measurement | Unit |
---|---|---|
tensile strength | aaaaa | aaaaa |
elongation at break | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com