Method for preparing damping material from waste polystyrene plastic foam and waste rubber powder
A waste polystyrene and foam technology, applied in the direction of plastic recycling, recycling technology, reagents, etc., can solve the problem of high cost, long process flow, and the application that affects the resource utilization of waste polystyrene foam and waste rubber powder, etc. Problems, to achieve the effect of low production cost, simple operation process and low equipment investment
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] 1. Prepare mixed solvents. Ethyl acetate and acetone were formulated as a mixed solvent for swelling waste polystyrene in a mass ratio of 4:1.
[0017] 2. Modified waste polystyrene. Put 10 grams of waste polystyrene that has been washed and dried into small pieces into a reactor, add 10 grams of the mixed solvent described in step 1, stir at normal temperature and pressure until dissolved, add 3 grams of epoxy resin, and condense at 70°C Reflux and stir evenly to obtain waste polystyrene modified material.
[0018] 3. Pretreatment of waste rubber powder. Plasticize the waste rubber powder on the open mill for 15 minutes, and use the shear force of the open mill to break and tear the rubber powder particles into small molecular segments.
[0019] 4. Mixing process. Take 100 grams of pretreated waste rubber powder, add the waste polystyrene modified material described in step 2, 5 grams of tackifier, 0.5 grams of anti-scorch agent, 0.5 grams of anti-aging agent, 1 gr...
Embodiment 2
[0022] 1. Prepare mixed solvents. Ethyl acetate and acetone were formulated as a mixed solvent for swelling waste polystyrene in a mass ratio of 3:1.
[0023] 2. Modified waste polystyrene. Put 15 grams of waste polystyrene that has been washed and dried into small pieces into the reactor, add 20 grams of the mixed solvent described in step 1, stir at normal temperature and pressure until dissolved, add 5 grams of epoxy resin, and condense at 70°C Reflux and stir evenly to obtain waste polystyrene modified material.
[0024] 3. Pretreatment of waste rubber powder. Plasticize the waste rubber powder on the open mill for 15 minutes, and use the shear force of the open mill to break and tear the rubber powder particles into small molecular segments.
[0025] 4. Mixing process. Take 100 grams of pretreated waste rubber powder, add the waste polystyrene modified material described in step 2, 5 grams of tackifier, 0.5 grams of anti-scorch agent, 0.5 grams of anti-aging agent, 1 ...
PUM
| Property | Measurement | Unit |
|---|---|---|
| damping ratio | aaaaa | aaaaa |
Abstract