Medical carbon dioxide absorbent soda lime and preparation method thereof
A technology of carbon dioxide and absorbent, applied in chemical instruments and methods, separation methods, and separation of dispersed particles, etc., can solve problems that are difficult to meet clinical needs, and achieve the effect of satisfying CO2 absorption rate, good friability, and not easy to dry
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0058] formula:
[0059] weight
[0060] Component (g)
[0061] Ca(OH) 2 500.00
[0062] NaOH 35.71
[0063] KOH 21.43
[0064] CaCl 2 2.86
[0065] Sodium carboxymethyl starch 21.43
[0066] Ethyl Violet 5.71
[0067] According to the above formula, mix Ca(OH)2, NaOH, KOH, humectant CaCl2 and pH indicating dye ethyl violet with 300g of water, then add disintegrant sodium carboxymethyl starch and water, the weight of water added is Ca (OH)2, NaOH, KOH, humectant CaCl2, 3% of the total weight of pH indicator dyeing agent ethyl violet and carboxymethyl starch sodium, made of soft material, extruded, and prepared as a diameter of 3mm and a height of 10mm The cylinder was dried at 110° C. for 3 hours to obtain a hard dry sample. After sieving to remove fine powder, water was sprayed on the obtained dry product until the weight content of water in the product was 17.8%, which was the product.
Embodiment 2
[0069] formula:
[0070] weight
[0071] Component (g)
[0072] Ca(OH) 2 500.00
[0073] NaOH 20.00
[0074] KOH 13.33
[0075] CaCl 2 6.67
[0076] Sodium carboxymethyl starch 33.33
[0077] Dadan Huang 6.67
[0078] According to the above formula, the Ca(OH) 2 , NaOH, KOH, CaCl 2 Add 290g of water to Dandanhuang, then add disintegrant CMS-Na and water, the weight of water added is Ca(OH)2, NaOH, KOH, moisturizing agent CaCl2, pH indicating dye ethyl violet and CMS-Na 3% of the total weight, made into a soft material, extruded, prepared into a cylinder with a diameter of 2.5mm and a height of 3mm, dried at 90°C for 4 hours to obtain a hard dry sample, sieved to remove fine powder, and then water Spray on the obtained dry product, the spraying amount of water is: until the weight content of water in the product is 13.0%, it is the product.
Embodiment 3
[0080] formula:
[0081] weight
[0082] Component (g)
[0083] Ca(OH) 2 500.00
[0084] NaOH 25.64
[0085] KOH 6.41
[0086] CaCl 2 3.85
[0087] Crospovidone 25.64
[0088] Dadan Yellow 0.025
[0089] The preparation method is the same as in Example 1, and the spraying amount of water is: until the weight content of water in the product is 11.80%, which is the product.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com