Unlock instant, AI-driven research and patent intelligence for your innovation.

Static-free glue and preparation method thereof

An anti-static and formulation technology, which is applied in adhesives, conductive adhesives, non-polymer adhesive additives, etc., can solve the problems of complex curing conditions, high price, and high cost, and achieve simple preparation process, strong practicability, The effect of strong adhesion

Active Publication Date: 2014-06-11
ARMY MEDICAL UNIV +1
View PDF4 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] At present, most of the antistatic adhesives reported at home and abroad use metal particles as fillers, such as nano-silver powder, flake gold powder, copper powder, etc. These materials are not only expensive, but also have migration phenomenon of metal particles, which will reduce their static electricity after long-term use. protective effect
Chinese patent CN1244558A discloses a kind of TiC engineering ceramic powder as conductive base material, SiO 2 It is an inorganic conductive adhesive that uses water glass or modified water glass as a curing agent as a filler, but its curing conditions are complicated, the cost is high, and it is brittle when used, so it is only suitable for bonding instruments and equipment, etc.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0027] First add 5g of hydroxyethyl cellulose to 335ml of water, stir for 10 minutes at a speed of 1200 rpm, then add 2.6g of cooked rubber powder, stir for 10 minutes at a speed of 1200 rpm, then add 41g of tung oil, and stir at a speed of 1200 rpm Stir at a speed of 10 minutes for 10 minutes to make ordinary glue. Then add 51.3g of conductive graphite into the above glue, and stir at a speed of 1300 rpm for 10 minutes to prepare the antistatic glue.

Embodiment 2

[0029] First add 8g of hydroxyethyl cellulose to 347.7ml of water, stir for 10 minutes at a speed of 1200 rpm, then add 4g of cooked rubber powder, stir for 10 minutes at a speed of 1200 rpm, then add 64g of tung oil, and stir at a speed of 1200 rpm Stir at a speed of 10 minutes for 10 minutes to make ordinary glue. Then add 24g of conductive carbon black into the above glue, and stir at a speed of 1300 rpm for 10 minutes to prepare the antistatic glue.

Embodiment 3

[0031] First add 4.7g of hydroxyethyl cellulose to 235ml of water, stir for 10 minutes at a speed of 1200 rpm, then add 2.3g of cooked rubber powder, stir for 10 minutes at a speed of 1200 rpm, then add 46.5g of tung oil, and stir at a speed of 1200 Stir at the speed of rev / min for 10 minutes to prepare common glue. Then add 46.5g of conductive zinc oxide into the above glue, and stir at a speed of 1300 rpm for 10 minutes to prepare the antistatic glue.

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention belongs to the technical field of chemical engineering, specifically components of static-free glue. The static-free glue comprises the following components in part by weight: 4.7-8 parts of cellulose, 2.3-4 parts of cooked glue powder, 41-64 parts of tung oil and 24-53.1 parts of conductive filler; the preparation method comprises the following steps of: adding the cellulose in the formula ratio to the water for sufficiently mixing uniformly to acquire cellulose solution, wherein the mass ratio of the cellulose to the water is (1.5-2.3) to 100; specifically, the preparation method is as follows: adding the coked glue powder to the cellulose solution, adding the tung oil in the formula ratio for sufficiently mixing after uniformly mixing to acquire the glue, wherein the acquired glue is added with conductive filler in the formula ratio, and then uniformly dispersed to acquire the static-free glue. The static-free glue has the characteristics of a simple preparation process, no poisonous and harmful substances, low cost, strong practicability and the like, and can be widely applied to performing electrostatic defending to a precise instrument, a life use, a building and the like.

Description

technical field [0001] The invention belongs to the technical field of chemical industry, and in particular relates to an antistatic glue and a preparation method thereof. Background technique [0002] With the advancement of science and technology and the wide use of various electrical equipment, the electromagnetic environment is becoming more and more complex in our daily life and industrial production. Many materials will generate static electricity during use. Excessive static electricity accumulation may cause extreme Terrible consequences, such as the human body may be injured by static electricity, the static electricity in the experimental environment that requires high cleanliness may generate dust and affect the experimental results, the electronic components of precision instruments may be damaged by static electricity breakdown, explosives, oil During the production, storage and transportation of high-risk items such as static electricity, sparks may cause combu...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C09J101/26C09J103/04C09J9/02C09J11/04
Inventor 张涛余争平高鹏周舟石小波王勇张红川
Owner ARMY MEDICAL UNIV