Embodiment 1
[0019] The novel leather retanning method of the present embodiment comprises the following steps:
[0020] 1) Take 100kg of wet blue hides and put them into the drum;
[0021] 2) Water washing: add 200kg of water at 40°C, 0.3kg of fatty acid glyceride, and rotate at 16rpm for 60min;
[0022] 3) Neutralization: Add 150kg of water at 35°C, 0.8kg of dye, rotate at 16rpm for 10min, add 2kg of aliphatic aldehyde, rotate at 16rpm for 30min, add 2kg of phenol syntan, rotate at 16rpm for 60min, make the pH value 4.8 ;
[0023] 4) Tanning: Add 50kg of water at 30°C, 2.5kg of dye, rotate at 16rpm for 30min, add 80kg of water at 50°C, 8kg of dicyandiamide resin tanning agent, rotate at 16rpm for 60min, add 1.5kg of formic acid, rotate at 16rpm 30min;
[0024] 5) Wash the skin with water at 20°C.
Embodiment 2
[0026] The novel leather retanning method of the present embodiment comprises the following steps:
[0027] 1) Take 100kg of wet blue hides and put them into the drum;
[0028] 2) Water washing: add 250kg of water at 40°C, 0.2kg of fatty acid glyceride, and rotate at 12rpm for 60min;
[0029] 3) Neutralization: Add 130kg of water at 35°C, 1kg of dye, rotate at 12rpm for 10min, add 2kg of aliphatic aldehyde, rotate at 12rpm for 30min, add 2.5kg of phenol syntan, rotate at 12rpm for 60min, make the pH value 5.0 ;
[0030] 4) Tanning: add 50kg of water at 30°C, 2kg of dye, rotate at 12rpm for 30min, add 80kg of water at 50°C, 10kg of melamine syntan, rotate at 12rpm for 60min, add 2kg of formic acid, and rotate at 12rpm for 30min;
[0031] 5) Wash with water at 25°C to remove the skin.
Embodiment 3
[0033] The novel leather retanning method of the present embodiment comprises the following steps:
[0034] 1) Take 100kg of wet blue hides and put them into the drum;
[0035] 2) Water washing: add 300kg of water at 40°C, 0.25kg of fatty acid glyceride, and rotate at 14rpm for 60min;
[0036] 3) Neutralization: Add 100kg of water at 35°C, 0.9kg of dye, rotate at 14rpm for 10min, add 2kg of aliphatic aldehyde, rotate at 14rpm for 30min, add 2.2kg of phenol syntan, rotate at 14rpm for 60min, make the pH value 4.9;
[0037] 4) Tanning: add 50kg of water at 30°C, 2.3kg of dye, rotate at 14rpm for 30min, add 80kg of water at 50°C, 9kg of naphthalene-based syntan, rotate at 14rpm for 60min, add 1.7kg of formic acid, and rotate at 14rpm for 30min ;
[0038] 5) Wash the skin at 22°C.
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com