A technology for interwoven fabrics and vehicles, which is applied in the field of preparation of vehicle interior fabrics, can solve the problems of burns to the human body, no deodorization and dust reduction functions, easy melting, etc., and achieves elimination of odor and odor, good application prospects, and melting small burn effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0024] Proceed as follows:
[0025] 1. Bamboo charcoal nylon filament is used as the outer layer of the fabric, and cotton yarn is used as the inner layer of the fabric.
[0026] 2. Use a double-sided circular knitting machine to weave the fabric into a composite cotton wool structure, ensuring that the two raw materials are respectively in the inner and outer layers of the fabric.
[0027] 3. Mix phosphate ester, titanate and acrylic acid at a mass ratio of 1:0.2:1.0 at a temperature of 50°C, and then add the above mixed solution and isopropyl to a container containing 800kg of warm water at 60°C. Alcohol, the mass ratio of the mixed solution to isopropanol is 10:1, stir for 30 minutes to prepare the flame retardant finishing working solution.
[0028] 4. Immerse the fabric in the flame retardant finishing working solution at 50°C for 3 hours to carry out flame retardant finishing on the fabric. During dipping, the fabric needs to be stirred continuously to ensure that the f...
Embodiment 2
[0034] Proceed as follows:
[0035] 1. Bamboo charcoal nylon filament is used as the outer layer of the fabric, and cotton yarn is used as the inner layer of the fabric.
[0036] 2. Use a double-sided circular knitting machine to weave the fabric into a composite cotton wool structure, ensuring that the two raw materials are respectively in the inner and outer layers of the fabric.
[0037] 3. Mix phosphate ester, titanate and acrylic acid at a mass ratio of 1:0.25:1.1 at a temperature of 55°C, and then add the above mixed solution and isopropyl to a container containing 900kg of warm water at 65°C. Alcohol, the mass ratio of the mixture to isopropanol is 11:1, stir for 35 minutes to prepare the flame retardant finishing working solution.
[0038]4. Immerse the fabric in the flame retardant finishing working solution at 55°C for 3.5 hours to carry out flame retardant finishing on the fabric. During dipping, the fabric needs to be stirred continuously to ensure that the flame ...
Embodiment 3
[0044] Proceed as follows:
[0045] 1. Bamboo charcoal nylon filament is used as the outer layer of the fabric, and cotton yarn is used as the inner layer of the fabric.
[0046] 2. Use a double-sided circular knitting machine to weave the fabric into a composite cotton wool structure, ensuring that the two raw materials are respectively in the inner and outer layers of the fabric.
[0047] 3. Mix phosphate ester, titanate and acrylic acid at a mass ratio of 1:0.3:1.2 at a temperature of 60°C, and then add the above mixed solution and isopropyl to a container containing 1000kg of warm water at 70°C. Alcohol, the mass ratio of the mixed solution to isopropanol is 12:1, and stirred for 40 minutes to obtain a flame retardant finishing working solution.
[0048] 4. Immerse the fabric in the flame-retardant finishing working solution at 60°C for 4 hours to carry out flame-retardant finishing on the fabric. During the dipping, the fabric needs to be stirred continuously to ensure t...