A zircon powder and coating technology, which is applied to casting molding equipment, coatings, casting molds, etc., can solve the problems of high radioactivity, physical injury of workshop employees, poor high temperature stability, etc., achieve good thixotropy and leveling, reduce The effect of cleaning workload and reducing porosity defects

Active Publication Date: 2013-08-28
SUZHOU XINGYE MATERIALS TECH
View PDF5 Cites 27 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] However, in recent years, the source of zircon powder has become more complicated, and the supply and demand relationship in the domestic and foreign markets has undergone significant changes, resulting in a rise in the price of zircon powder.
In addition, domestically processed zircon powder is generally ground by Raymond mills, which has high impurity content and high radioactivity, which is likely to cause physical harm to workshop employees.
Cast steel coatings currently on the market, in addition to zircon powder coatings, also have high-alumina bauxite coatings, chrome ore powder coatings, etc., but these coatings have poor high temperature stability and are difficult to meet the requirements of cast steel.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Zircon power alternative coating for casting and preparation method thereof
  • Zircon power alternative coating for casting and preparation method thereof
  • Zircon power alternative coating for casting and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0054] Example 1 Preparation of zircon powder substitute coating for foundry

[0055]

[0056] The preparation method is as follows:

[0057] (1) Add organic bentonite to toluene to make a paste to form a semi-finished product A.

[0058] (2) Add semi-finished product A, attapulgite, thermoplastic phenolic resin, rosin, 325 mesh white corundum powder, and 325 mesh andalusite powder into the kneader in this order, and knead for 1 hour to form semi-finished product B.

[0059] (3) Add isopropanol and ethanol to the high-speed disperser, then add semi-finished product B, stir at 1000 rpm, and stir for 1 hour to form semi-finished product C.

[0060] (4) Pass the semi-finished product C through a colloid mill, and the glue is ground into a slurry, and then packed in barrels.

[0061] The new cast steel coating has high refractoriness and good sintering peeling performance, and the surface quality of cast steel parts is greatly improved.

Embodiment 2

[0062] Example 2 Preparation of Zircon Powder Substitute Coating for Casting

[0063] The composition of the new cast steel coating: isopropanol 10%, toluene 3%, ethanol 6.0%, organic bentonite 1.3%, attapulgite 1.0%, thermoplastic phenolic resin 0.8%, rosin 0.3%, 325 mesh white corundum powder 40%, 325 mesh Andalusite powder 37.6%.

[0064] The new cast steel coating has high refractoriness and good sintering peeling performance, and the surface quality of cast steel parts is greatly improved.

Embodiment 3

[0065] Example 3 Preparation of Zircon Powder Substitute Coating for Casting

[0066] The composition of the new cast steel coating: isopropanol 6%, toluene 3.5%, ethanol 9%, organic bentonite 1.5%, attapulgite 1.1%, thermoplastic phenolic resin 0.7%, rosin 0.4%, 325 mesh white corundum powder 55%, 325 mesh Andalusite powder 22.8%.

[0067] The new cast steel coating has low cost, no radioactivity, good fluidity and good sintering peeling performance, and the surface quality of the steel casting is greatly improved.

[0068]

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
particle sizeaaaaaaaaaa
particle sizeaaaaaaaaaa
Login to view more

Abstract

The invention discloses a zircon power alternative coating for casting, which is characterized in that a coating composition comprises carrier liquid consisting of isopropyl alcohol, toluene and ethanol, a suspending agent consisting of organobentonite and attapulgite, an adhesive consisting of thermoplastic phenolic resin and rosin, and refractory aggregate consisting of white alundum powder and andalusite powder. The coating composition comprises the following components by weight percent: 6-10 percent of isopropyl alcohol, 2-4 percent of toluene, 6-10 percent of ethanol, 0.5-1.5 percent of organobentonite, 1-2 percent of attapulgite, 0.2-1.0 percent of thermoplastic phenolic resin, 0.2-1.0 percent of rosin, 15-55 percent of white alundum powder and 15-55 percent of andalusite powder. Compared with the conventional common cast steel zircon power coating, the coating has high thixotropy and leveling property, is smooth and dense and has enough normal temperature and high-temperature strength, so that the casting roughness meets the quality requirement; and moreover, the zircon power alternative coating is low in gas outlet quantity and has proper shielding property, and the defects of the casting air holes can be obviously reduced.

Description

technical field [0001] The invention belongs to the technical field of casting coating and its synthesis process, and in particular relates to a zircon powder substitute coating for casting and a preparation method thereof. Background technique [0002] The chemical composition of zircon powder is ZrO 2 >65%, SiO 2 <33%, TiO 2 <0.4%, Fe 2 o 3 <0.5%, P 2 o 5 <0.5%, Al 2 o 3 <0.3%; Particle size: 95% pass 320 mesh, the rest pass 260 mesh. Required refractoriness: not less than 1550°C; total radioactive specific activity not greater than 2*10 -6 Ci·kg -1 ; Commonly used as a mold coating in the investment casting industry. Zircon powder is not only used as the main material in the ceramic industry, but also used for glazing, which increases the wear resistance and surface finish of the made ceramics. Zircon powder has specialized uses in many chemical industries, including cosmetics, cement, food preservation, tanning, fibers (for making flame reta...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): B22C3/00
Inventor 王进兴金车陆玉峰王文浩王锦程陈亚东
Owner SUZHOU XINGYE MATERIALS TECH
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products