Alcohol-based resin coating
A technology of alcohol-based resin and coating, applied in the direction of coating, etc., can solve the problems of affecting the environment and causing great harm, and achieve the effect of good drying, good transferability, and neat edges of transferred characters
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0011] Rosin improved phenolic resin: take 2100 parts of p-octylphenol to dissolve, add 90 parts of 25% caustic soda solution, 160 parts of 37% formaldehyde, and react at 55°C for 8 hours to obtain the initial condensation product of phenolic resin; take 750 parts of rosin, Malay 30 parts of acid anhydride and 250 parts of initial condensate of phenolic resin were placed in a reactor, under the protection of nitrogen flow, stirred and reacted at 180-200°C for 3 hours, then added 106 parts of pentaerythritol and 16 parts of glycerin, and reacted at 200-270°C until acid When the value reaches 15-20, the rosin-improved phenolic resin is obtained.
[0012] Alcohol-based resin coating: Take 17 parts of rosin modified phenolic resin, 7 parts of kaolin, 10 parts of carbon black, 0.2 parts of preservative (such as SJ1006 of Tengzhou Anticorrosion Technology Co., Ltd.), 0.4 parts of dispersant (such as BYK K-163) , 36 parts of ethanol, 5 parts of isopropanol. First heat and dissolve t...
Embodiment 2
[0014] Alcohol-based resin paint: Take 15 parts of rosin-improved phenolic resin, 5 parts of sodium carbonate, 6 parts of pigment, 0.1 part of preservative, 0.3 part of dispersant, and 50 parts of ethanol. First heat and dissolve the rosin-improved phenolic resin in ethanol, then add other components in sequence, and use a grinder to disperse the system evenly, and the particle size should be below 10 μm.
Embodiment 3
[0016] Alcohol-based resin coating: 20 parts of rosin modified phenolic resin, 10 parts of aluminum hydroxide, 15 parts of pigment, 0.3 part of preservative, 0.5 part of dispersant, 40 parts of n-butanol. First heat and dissolve rosin-modified phenolic resin in n-butanol, then add other components in sequence, and use a grinder to disperse the system evenly, and the particle size should be below 10 μm.
PUM
Property | Measurement | Unit |
---|---|---|
softening point | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com