Embodiment 1
[0085] A closed coating process for wood furniture, comprising the following steps:
[0086] (1) Use self-drying resin, coating agent and thinner to prepare hand-swept coating agent, wherein the mass percentages of self-drying resin, coating agent and thinner are: 10%, 60 and 30% respectively;
[0087] (2) Sweep and coat the hand-swept coating agent on the workpiece, and the coating amount is controlled at 80g / m 2 ;
[0088] (3) Start the mobile UV dryer, and dry the coating agent through the movement of the mobile UV dryer;
[0089] (4) After diluting the sealing coating agent, sweep it on the workpiece;
[0090] (5) Start the mobile UV dryer, and dry the coating agent through the movement of the mobile UV dryer.
[0091] Wherein, the self-drying resin is a medium-temperature curing agent tert-butyl peroxide-2-ethylhexanoate, acrylic resin and ethyl ester; the diluent is one or both of ethyl ester and ethanol; the film coating agent is an application Products described in...
Embodiment 2
[0095] A closed coating process for wood furniture, comprising the following steps:
[0096] (1) Use self-drying resin, coating agent and thinner to prepare hand-swept coating agent, wherein the mass percentages of self-drying resin, coating agent and thinner are: 35%, 60% and 5% respectively ;
[0097] (2) Sweep the hand-swept coating agent on the workpiece, and the coating amount is controlled at 120g / m 2 ;
[0098] (3) Start the mobile UV dryer, and dry the coating agent through the movement of the mobile UV dryer;
[0099] (4) After diluting the sealing coating agent, sweep it on the workpiece;
[0100] (5) Start the mobile UV dryer, and dry the coating agent through the movement of the mobile UV dryer;
[0101] Wherein, the self-drying resin includes medium-temperature curing agent tert-butyl peroxide-2-ethylhexanoate, acrylic resin and ethyl ester; the diluent is one or both of ethyl ester and ethanol; the coating agent is an application Products described in Chines...
Embodiment 3
[0108] A closed coating process for wood furniture, comprising the following steps:
[0109] (1) Use self-drying resin, coating agent and thinner to prepare hand-swept coating agent, wherein the mass percentages of self-drying resin, coating agent and thinner are: 10%, 85% and 5% respectively ;
[0110] (2) Sweep and coat the hand-swept coating agent on the workpiece, and control the coating amount at 100g / m 2 ;
[0111] (3) Start the mobile UV dryer, and dry the coating agent through the movement of the mobile UV dryer;
[0112] (4) After diluting the sealing coating agent, sweep it on the workpiece;
[0113] (5) Start the mobile UV dryer, and dry the coating agent through the movement of the mobile UV dryer;
[0114] Wherein, the self-drying resin includes medium-temperature curing agent tert-butyl peroxide-2-ethylhexanoate, acrylic resin and ethyl ester; the diluent is one or both of ethyl ester and ethanol; the coating agent is an application The product described in ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com