A kind of antibacterial, moisture-conducting and anti-ultraviolet bamboo dyer blended yarn
An anti-ultraviolet and bamboo dale technology, applied in the field of yarn, can solve the problems of fabric handle, poor air permeability, poor anti-ultraviolet effect, poor fiber spinnability, etc., to achieve good moisture absorption, air permeability and drape, and improve wearing comfort. , strong antibacterial effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0029] Raw material preparation: Bamboo dale fiber 0.8dtex×38mm
[0030] Moisture-wicking and UV-resistant super-spun cotton fiber 0.9dtex×38mm
[0031] The cross-section of the moisture-wicking and anti-ultraviolet super-spun cotton fiber is cross-shaped, and 0.8% nano-scale titanium dioxide powder is added to the spinning polymer mass during the spinning process.
[0032] Yarn Spec: Bamboo Dyer / Wicking & UV Resistant Superspun Cotton 30 / 70
[0033] 13.8tex, twist factor 280
[0034] The production process is as follows:
[0035] (1) Cleaning process:
[0036] Adoption process: FA002A type plucking machine → SFA035C type mixed cotton opener → FA025 type multi-compartment cotton blender → FA106A type porcupine opener → SFA161 type vibrating cotton feeder → A076F type lapping machine.
[0037] The bamboo dale fiber of the present invention, moisture-absorbing perspiration and anti-ultraviolet super-spun cotton fibers have good regularity, few impurities, smooth fiber surfac...
Embodiment 2
[0049] Raw material preparation: bamboo dale fiber 0.9dtex×38mm
[0050] Moisture-wicking and UV-resistant super-spun cotton 0.9dtex×38mm
[0051] The cross-section of the moisture-wicking and anti-ultraviolet super-spun cotton fiber is cross-shaped, and 1.2% nano-scale titanium dioxide powder is added to the spinning polymer mass during the spinning process.
[0052] Yarn Spec: Bamboo Dyer / Wicking & UV Resistant Superspun Cotton 40 / 60
[0053] 13.8tex, twist factor 320
[0054] Spinning process:
[0055] (1) Cleaning process: After mixing the fibers according to the proportion, follow the principle of short process, low speed, less beating and less shedding, and the basis weight of the cotton lap is 380g / m;
[0056] (2) Carding process: cylinder speed is 310r / min, licker-in speed is 750r / min, doffer speed is 24r / min, cylinder doffer gauge is 0.12mm, raw sliver weight is 18.5g / 5m;
[0057] (3) Drawing process: adopt two merging, 8 slivers are merging, the drafting ratio of...
Embodiment 3
[0062] Raw material preparation: bamboo dale fiber 1.2dtex×38mm
[0063] Moisture-wicking and UV-resistant super-spun cotton 1.2dtex×38mm
[0064] The cross-section of the moisture-wicking and anti-ultraviolet super-spun cotton fiber is cross-shaped, and 2.2% of the mass of the spinning polymer is added with nano-scale titanium dioxide powder during the spinning process.
[0065] Yarn Spec: Bamboo Dyer / Wicking Anti-UV Superspun Cotton 50 / 50
[0066] 27.8tex, twist coefficient 360
[0067] The spinning process is the same as in Example 1.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com