A sand-fixing agent and chemical technology, which is applied in the field of chemical sand-fixing agent preparation, can solve problems such as environmental pollution, high cost, and long process time, and achieve the effects of reducing cost, reducing process production time, and reducing pollution
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] Example 1 The preparation steps of chemical sand-fixing agent are as follows:
[0017] (1) Heat 5g of polyvinyl alcohol powder and 95g of water to 80°C for 30 minutes to completely dissolve the polyvinyl alcohol and prepare 5wt% polyvinyl alcohol;
[0018] (2) Dissolve 5g of polyacrylamide in 95g of warm water at 40°C, drop it into (1) through a burette (control the titration speed, titrate slowly), keep the temperature at 75°C, and stir for 20 minutes;
[0019] (3) Take 33ml of silica sol and drop it into (2) through a burette (control the titration speed, titrate slowly), keep the temperature at 75°C, and stir for 20 minutes;
[0020] (4) Dissolve 3-4g of nano-scale calcium carbonate solid in 96-97g of water (3%-4% nano-scale calcium carbonate dispersion), and slowly drop into (3) through the burette (control the titration speed, slow titration), Constant temperature 75°C, stirring for 20 minutes;
[0021] (5) Add 5g of sodium tetraborate directly to the above mixtu...
Embodiment 2
[0023] Example 2 The preparation steps of chemical sand-fixing agent are as follows:
[0024] (1) Mix 8g of polyvinyl alcohol powder with 92g of water, heat to 80°C for 30 minutes to completely dissolve the polyvinyl alcohol, and prepare 8wt% polyvinyl alcohol;
[0025] (2) Dissolve 8g of polyacrylamide in 92g of warm water at 41°C, slowly add the above mixture (control the titration speed, titrate slowly), keep the temperature at 78°C, and stir for 25 minutes;
[0026] (3) Take 32ml of silica sol and slowly add it to (2) (control the titration speed, titrate slowly), keep the temperature at 78°C, and stir for 25 minutes;
[0027] (4) Dissolve 3-4g of nano-scale calcium carbonate solid in 96-97g of water (3%-4% nano-scale calcium carbonate dispersion), and slowly add to (3) (control titration speed, slow titration), constant temperature 78 ℃, stirring for 25 minutes;
[0028] (5) Add 8g of sodium tetraborate directly into (4), keep the temperature at 78°C, and stir for 24 mi...