Cow leather dyeing process
A process, cowhide technology, applied in dyeing method, small raw hide/large raw hide/leather/fur treatment, small raw hide/large raw hide/leather hide/fur chemical treatment, etc. Significant and other problems, to achieve the effect of easy operation and good color fixing
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] A dyeing process for cowhide, including the following steps:
[0020] A. Backwater: First add 100% water to the drum, add 9% industrial salt, rotate for 20 minutes, control the Baume degree to 8, and then subcutaneously add 0.3% degreasing agent and 4% small Soda, rotate for 20 minutes, adjust the pH to 6.8, drain;
[0021] B. Retanning: Add 50% water, 0.5% dye amount, 0.2% dye auxiliaries, and rotate for 15 minutes into the drum; add 0.6% formic acid, control pH 3.5, rotate for 15 minutes, and add 3% chrome powder, rotate for 60 minutes ; Add 1.0% of sodium formate and 0.3% of baking soda, rotate for 30 minutes, drain and wash with water;
[0022] C. Filling and dyeing: first add 80% water, TRS 2%, macromolecular acrylic 3%, rotating for 40 minutes in the drum; NE 1.5%, DM 3%, rotating for 40 minutes; PR 2%, tannin extract 1%, dye 0.7 %, dye auxiliaries 0.2%, rotate for 60 minutes; finally add 0.8% formic acid, rotate for 30 minutes;
[0023] D. Add fat: make up water unt...
Embodiment 2
[0025] A dyeing process for cowhide, including the following steps:
[0026] A. Backwater: First add 110% water to the drum, add 11% industrial salt, rotate for 20 minutes, control the Baume degree to 8.5, and then subcutaneously add 0.5% degreasing agent and 6% small Soda, rotate for 20 minutes, adjust the pH to 7.0, and drain;
[0027] B. Retanning: first add 60% water, 0.6% dye amount, 0.4% dye auxiliaries, and rotate 15 minutes into the drum; add 0.9% formic acid, control pH 3.8, rotate 15 minutes, add 6% chrome powder, rotate 60 minutes ; Add 2.0% sodium formate, 0.35% baking soda, rotate for 30 minutes, drain and wash with water;
[0028] C. Filling and dyeing: first add 90% water, TRS4%, macromolecular acrylic acid 3% to the drum, rotate for 40 minutes; NE 2.0%, DM 4%, rotate for 40 minutes; PR2.5%, tannin extract 2%, dye 1.0 %, dye auxiliaries 0.3%, rotate for 60 minutes; finally add 0.9% formic acid, rotate for 30 minutes;
[0029] D. Filling: add water to a material-to-...
Embodiment 3
[0031] A dyeing process for cowhide, including the following steps:
[0032] A. Backwater: First add 105% water to the drum, add industrial salt 10%, rotate for 20 minutes, control the Baume degree to 8.3, and then subcutaneously add 0.4% degreasing agent and 5% small Soda, rotate for 20 minutes, adjust the pH to 7.0, and drain;
[0033] B. Retanning: first add 55% water, 0.55% dye amount, 0.3% dye auxiliaries to the drum, rotate for 15 minutes; add 0.75% formic acid, control pH 3.6, rotate for 15 minutes, add 4.5% chromium powder, rotate for 60 minutes ; Add 1.5% sodium formate and 0.33% baking soda, rotate for 30 minutes, drain and wash with water;
[0034] C. Filling and dyeing: first add 85% water, 3% TRS, 3% macromolecular acrylic acid to the drum, rotating for 40 minutes; NE 1.75%, DM 3.5%, rotating for 40 minutes; PR 2.3%, tannin extract 1.5%, dye 0.9 %, dye auxiliaries 0.25%, rotate for 60 minutes; finally add 0.8% formic acid, rotate for 30 minutes;
[0035] D. Filling: ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com