A bedding and production method technology, applied in the field of bedding, can solve the problems of affecting the mechanical properties of materials, shortening the product life, poor binding force, etc., and achieve the effect of long-lasting and stable negative ion release, good mechanical properties, and good dispersibility
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0037] Add 100 parts of polyether polyol, 2.0 parts of silicone oil, 3.6 parts of water, 0.2 parts of tertiary amine catalyst, and 0.1 part of stannous octoate catalyst into reaction vessel A, stir at a high speed evenly and set aside.
[0038] In reaction vessel B, 25 parts of TDI, 5 parts of negative ion mineral powder were added under high-speed stirring, reacted at 40°C for 1 hour, and then set aside.
[0039] After mixing the materials in A and B reaction containers for 1 minute, immediately pour them into a mattress mold for foaming, and release the mold after aging to obtain a polyurethane mattress that can release negative ions.
[0040] After testing, the negative ion release amount of the polyurethane mattress is 2000 / cm3.
Embodiment 2
[0042] Add 100 parts of polyether polyol, 2.5 parts of silicone oil, 2.0 parts of water, 0.8 parts of tertiary amine catalyst, and 0.4 part of stannous octoate catalyst into reaction vessel A, stir at a high speed until uniform, and set aside.
[0043] In the reaction vessel B, 40 parts of MDI, 10 parts of negative ion mineral powder were added under high-speed stirring, and reacted at 70°C for 3 hours before use.
[0044] After mixing the materials in A and B reaction containers for 5 minutes, immediately pour them into pillow molds for foaming, and release them after aging to form a polyurethane pillow that can release negative ions.
[0045] After testing, the negative ion release capacity of the polyurethane pillow is 3000 / cm3.