Method for modifying printing ink by adding colophony polyol ester
A technology of rosin polyol ester and ink, which is applied in the directions of ink, household utensils and applications, can solve the problems of long duration, large residual amount, endangering the health of users, etc., and achieves the effect of low cost and wide source of raw materials
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] Put 20% water, 25% vegetable oil, 15% ethanolamine, 0.5% organic silicon defoamer and 1% soybean lecithin wetting agent into a dispersion cylinder, and disperse evenly at 500r / min for 2 Hours, after the dispersion is even, the liquid is filtered, and the filtered emulsion is put into the dispersion tank again, and 25% water-soluble acrylic resin, 10% water-based acrylic color paste and 3% rosin polyol ester are added successively, according to 600r / Min speed, disperse evenly for 4 hours, finally add 0.5 parts of silicone defoamer and filter, then you can get an ink with strong adhesion and stable performance.
Embodiment 2
[0017] Put 20% water, 25% vegetable oil, 15% ethanolamine, 0.5% organic silicon defoamer and 1% soybean lecithin wetting agent into a dispersing cylinder, and disperse evenly at a speed of 600r / min for 1 Hours, after the dispersion is even, the liquid is filtered, and the filtered emulsion is put into the dispersion tank again, and 25% water-soluble acrylic resin, 10% water-based acrylic color paste and 3% rosin polyol ester are added successively, according to 600r / Min speed, disperse evenly for 4 hours, finally add 0.5 parts of silicone defoamer and filter, then you can get an ink with strong adhesion and stable performance.
Embodiment 3
[0019] Put 20% water, 25% vegetable oil, 15% ethanolamine, 0.5% organic silicon defoamer and 1% soybean lecithin wetting agent into a dispersion cylinder, and disperse evenly at 500r / min for 2 hour, after the dispersion is uniform, the liquid is filtered, and the filtered emulsion is put into the dispersion tank again, and 25% of water-soluble acrylic resin, 10% of water-based acrylic color paste and 3% of rosin polyol ester are added successively, according to 800r / min speed, disperse evenly for 2 hours, and finally add 0.5 parts of silicone defoamer and filter to get an ink with strong adhesion and stable performance.