A catalyst for denitrification and demercuration of coal-fired flue gas and its preparation method and application
A coal-fired flue gas and catalyst technology, applied in chemical instruments and methods, physical/chemical process catalysts, separation methods, etc., can solve the problems of industrialization difficulties, catalysts are easy to poison, high cost and difficult industrialization, etc., and achieve high efficiency and reduce equipment cost effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0036] Example 1: MnO 2 -MoO 3 / ATP preparation
[0037] (1) Weigh 20g of attapulgite (ATP) into 200mL of distilled water and stir evenly. Under the action of a certain temperature and high shear force, add a certain concentration of sodium hexametaphosphate aqueous solution. After stirring for a period of time, the mixed solution Perform ultrasonic dispersion for a certain period of time, let stand, decant the supernatant suspension, centrifuge the obtained solid, wash it with double distilled water until it is neutral, and dry it at a certain temperature to obtain pure attapulgite.
[0038] (2) Weigh 4g of pure attapulgite and 0.4mmol of ammonium molybdate into 100ml of distilled water and stir evenly, then add 0.08mmol of cetyltrimethylammonium bromide and stir well, then adjust the pH value to 3.5 with glacial acetic acid , and then use nitric acid to bring the pH value to 1, stir for 10 minutes, and ultrasonically oscillate for 30 minutes.
[0039] (3) Add 0.5 g of sod...
Embodiment 2
[0048] Example 2: CeO 2 -MoO 3 / ATP preparation
[0049] (1) Weigh 20g of attapulgite (ATP) into 200mL of distilled water and stir evenly. Under the action of a certain temperature and high shear force, add a certain concentration of sodium hexametaphosphate aqueous solution. After stirring for a period of time, the mixed solution Perform ultrasonic dispersion for a certain period of time, let stand, decant the supernatant suspension, centrifuge the obtained solid, wash it with double distilled water until it is neutral, and dry it at a certain temperature to obtain pure attapulgite.
[0050] (2) Weigh 4g of pure attapulgite and 0.4mmol of ammonium molybdate into 100ml of distilled water and stir evenly, then add 0.08mmol of cetyltrimethylammonium bromide and stir well, then adjust the pH value to 3.5 with glacial acetic acid , and then use nitric acid to bring the pH value to 1, stir for 10 minutes, and ultrasonically oscillate for 30 minutes.
[0051] (3) Add 0.5 g of sod...
Embodiment 3
[0060] Example 3: ZrO 2 -MoO 3 / ATP preparation
[0061] (1) Weigh 20g of attapulgite (ATP) into 200mL of distilled water and stir evenly, under the action of a certain temperature and high shear force, add a certain concentration of sodium hexametaphosphate aqueous solution, after stirring for a period of time, the mixed solution Perform ultrasonic dispersion for a certain period of time, let stand, decant the upper suspension, centrifuge the obtained solid, wash it with double distilled water to neutrality, and dry it at a certain temperature to obtain pure attapulgite.
[0062] (2) Weigh 4g of pure attapulgite and 0.4mmol of ammonium molybdate into 100ml of distilled water and stir evenly, then add 0.08mmol of cetyltrimethylammonium bromide and stir well, then adjust the pH value to 3.5 with glacial acetic acid , and then use nitric acid to bring the pH value to 1, stir for 10 minutes, and ultrasonically oscillate for 30 minutes.
[0063] (3) Add 0.5 g of sodium acetate,...
PUM