Preparation method of nano silver tri-proof antibacterial finishing agent

A technology of antibacterial finishing agent and three-proof finishing agent, which is applied in the direction of fiber treatment, liquid repellent fiber, anti-coloring pollution/anti-fouling fiber, etc. It can solve the problems of dispersibility, poor stability, easy agglomeration, etc., and achieve Not easy to agglomerate, good dispersion, simple process effect

Active Publication Date: 2016-05-11
SIMMONS BEDDING&FURNITURE (SUZHOU) LTD
View PDF6 Cites 1 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

However, there are still some problems with nano silver at present: the dispersion and stability are relatively poor, and it is easy to agglomerate

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Preparation method of nano silver tri-proof antibacterial finishing agent

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0028] The first step is the preparation of nano-silver coated with modified starch, the method is as follows:

[0029] (1) the silver nitrate solution of preparation 0.05mol / L and the sodium citrate solution that concentration is 1% are subsequent use;

[0030] (2) Add 50ml of water into the three-necked flask, then add 0.25g of modified starch, turn on the heat-collecting constant temperature heating magnetic stirrer, put the above three-necked flask into it, stir and heat up to 95°C for about 30min to gelatinize the starch;

[0031] (3) Lower the temperature to 70°C, add dropwise 10ml of the prepared silver nitrate solution into the three-necked flask, and continuously stir for 10 minutes;

[0032] (4) Add 2ml of the prepared sodium citrate solution dropwise at a rate of 1 drop / s, and stir to make it fully react;

[0033] (5) After the color of the reaction system no longer changes, that is, after the reaction is sufficient, the prepared sol is taken out from the reaction ...

Embodiment 2

[0038] The first step is the preparation of nano-silver coated with modified starch, and its preparation steps and process are the same as in Example 1.

[0039] The second step is to prepare nano-silver three-proof antibacterial finishing agent according to the optimization results of each component, as follows: (1) according to nano-silver sol: HS1100:ATB9800:TPM9007=0.3:7:2:3, weigh 3g of nano-silver sol , HS1100 three-proof finishing agent 70g, ATB9800 antibacterial finishing agent 20g, TPM9007 antibacterial finishing agent 30g (total liquid weight 1000g)

[0040] (2) First place 70g of HS1100 three-proof finishing agent in a three-necked flask with stirring, then gradually add 3g of nano-silver sol, 20g of ATB9800 antibacterial finishing agent, 30g of TPM9007 antibacterial finishing agent, and add water to a total liquid weight of 1000g.

[0041] (3) Stir the compounded three antibacterial agent at normal temperature and pressure for 10 minutes until it is uniform.

Embodiment 3

[0043] The first step is the preparation of nano-silver coated with modified starch, and its preparation steps and process are the same as in Example 1.

[0044] The second step is to prepare nano-silver three-proof antibacterial finishing agent according to the optimization results of each component, as follows: (1) according to nano-silver sol: HS1100:ATB9800:TPM9007=0.4:8:3:3, weigh 4g of nano-silver sol , HS1100 three-proof finishing agent 80g, ATB9800 antibacterial finishing agent 30g, TPM9007 antibacterial finishing agent 30g (total liquid weight 1000g)

[0045] (2) First place 80g of HS1100 three-proof finishing agent in a three-necked flask with stirring, then gradually add 4g of nano-silver sol, 30g of ATB9800 antibacterial finishing agent, 30g of TPM9007 antibacterial finishing agent, and add water to a total liquid weight of 1000g.

[0046] (3) Stir the compounded three antibacterial agent at normal temperature and pressure for 10 minutes until it is uniform.

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
antibacterial rateaaaaaaaaaa
antibacterial rateaaaaaaaaaa
antibacterial rateaaaaaaaaaa
Login to View More

Abstract

The invention discloses a nano silver tri-proof antibacterial finishing agent and a preparation method thereof. The nano silver tri-proof antibacterial finishing agent is prepared from nano silver antibacterial sol coated by modified starch, a tri-proof finishing agent HS1100, an antibacterial finishing agent ATB9800 and an antibacterial finishing agent TPM9007 according to a weight ratio of 0.1-0.4:5-9:2-5:2-4. Naturally degradable polymer-starch is used as a protective agent and a dispersing agent, and the nano silver sol coated by the starch is prepared by adopting a simple liquid-phase chemical reduction method, so that the nano silver tri-proof antibacterial finishing agent is simple in process, environment friendly, high in dispersity and less prone to aggregation. The nano silver tri-proof antibacterial finishing agent prepared by the method can be used for one-bath finishing, and is simple in process and convenient to operate compared with split-bath finishing.

Description

[0001] This application is a divisional application with application number: 201410606498.6, application date: 2014.10.31, and name "nano-silver three-proof antibacterial finishing agent and its preparation method". technical field [0002] The invention relates to a preparation method of a nano-silver three-proof antibacterial finishing agent. Background technique [0003] With the improvement of people's quality of life, single-function textiles are increasingly unable to meet people's needs. In some special occasions, there are more requirements (such as waterproof, oil-proof, anti-fouling, anti-ultraviolet, anti-static, antibacterial properties, etc.) ), which makes the development of multifunctional textiles more and more people's attention. At present, the three-proof antibacterial finishing generally adopts the three-proof antibacterial separate bath finishing, that is, the first three-proof and then the anti-bacterial finishing or the first anti-bacterial and then th...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): D06M23/00D06M11/83D06M15/00
CPCD06M11/83D06M15/00D06M23/00D06M2200/01D06M2200/11D06M2200/12
Inventor 崔建伟陈凤卞晨霞张华陈春升
Owner SIMMONS BEDDING&FURNITURE (SUZHOU) LTD