Method of preparing anti-pilling finishing liquid for worsted tweed
A tweed, anti-pilling technology, applied in fiber processing, textiles and papermaking, abrasion-resistant fibers, etc., can solve problems such as pilling, and achieve the effect of reducing dosage and directional friction effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] For realizing above-mentioned technical effect, the preparation method of worsted tweed anti-pilling finishing solution in embodiment 1 comprises the following steps:
[0019] S1: Prepare the swelling agent solution, dissolve the wool swelling agent in deionized water, and introduce the mixed solution into the reaction vessel;
[0020] S2: Extract wool keratin, add thioglycolic acid to the mixed solution in the reaction vessel to make an extract, pass inert gas protection, heat to 50°C, add shredded wool in batches under heat preservation, heat to 87°C, and keep warm for 90 minutes ;
[0021] S3: inert oxide stable solution, add fumed silica into the reaction vessel in S2, and keep stirring for 15 minutes;
[0022] S4: Add hypophosphorylated tris(propyl alcohol) phosphine hydrogen phosphine ionic liquid to the mixed solution obtained in S3, and adjust the pH value to 4.5 with citric acid to prepare worsted tweed anti-pilling finishing solution.
[0023] The addition a...
Embodiment 2
[0029] The difference between embodiment 2 and embodiment 1 is:
[0030] In S2, heat the extract to 60°C, add shredded wool in batches under heat preservation, heat to 95°C, and keep warm for 150 minutes;
[0031] S3: Add fumed silica to the reaction vessel in S2, and keep stirring for 25 minutes;
[0032] S4: Add hypophosphorylated tris(propyl alcohol) phosphine hydrogen phosphine ionic liquid to the mixed solution obtained in S3, and adjust the pH value to 5.5 with citric acid to prepare worsted tweed anti-pilling finishing solution.
[0033] The addition amount of hypophosphorylated tri(propyl alcohol) phosphine hydrogen phosphine ionic liquid in worsted tweed anti-pilling finishing solution is 22%.
[0034] The wool swelling agent is urea, and the molar concentration of the wool swelling agent in the mixed solution in S1 is 6mol / L.
[0035] The molar volume ratio of the addition of mercaptoacetic acid to the mixed solution is 8mol / L.
[0036] The ratio of the total weig...
Embodiment 3
[0039] The difference between embodiment 3 and embodiment 1 is:
[0040] In S2, heat the extract to 55°C, add shredded wool in batches under heat preservation, heat to 91°C, and keep warm for 115 minutes;
[0041] S3: Add fumed silica to the reaction vessel in S2, and keep stirring for 20 minutes;
[0042] S4: Add hypophosphorylated tris(propyl alcohol) phosphine hydrogen phosphine ionic liquid to the mixed solution obtained in S3, and adjust the pH value to 5 with citric acid to prepare worsted tweed anti-pilling finishing solution.
[0043] The addition amount of hypophosphorylated tri(propyl alcohol) phosphine hydrogen phosphine ionic liquid in worsted tweed anti-pilling finishing solution is 19%.
[0044] The wool swelling agent is a 1:1 composition of lithium chloride and urea, and the molar concentration of the wool swelling agent in the mixed solution in S1 is 4mol / L.
[0045] The molar volume ratio of the addition of mercaptoacetic acid to the mixed solution is 4mol / ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com