A preparation process of flexible nitrile double-sided adhesive fire hose
A fire hose and a preparation technology, applied in the direction of rubber layered products, layered products, chemical instruments and methods, etc., can solve the problems of low adhesive strength of the reinforcement layer, affect the use experience, stiff hand feeling, etc., and reach the service life Long, well-selected materials, good bending resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0040] The preparation technology of a kind of flexible nitrile double-sided adhesive fire hose described in the present embodiment comprises the following steps:
[0041] (1) Prepare raw materials:
[0042] Percentage by weight includes NBR / PVC7030: 46%, silica: 17%, plasticizer oil: 10%, activator: 3%, stearic acid: 0.5%, vulcanizing agent: 0.5%, accelerator: 1%, Calcium Carbonate: 20%, Methyl Donor: 1%, Methylene Donor: 1%;
[0043] (2) Rubber mixing:
[0044] One stage: use internal mixer, pass cooling water,
[0045] Ingredients Temperature
[0046] NBR / PVC7030 70℃
[0047] Active agent + 1 / 3 white carbon black + 1 / 3 calcium carbonate + methyl donor 80°C
[0048] 1 / 3 white carbon black + 1 / 3 calcium carbonate + 1 / 2 plasticizer oil 95℃
[0049] 1 / 3 white carbon black + 1 / 3 calcium carbonate + 1 / 2 plasticizer oil 110℃
[0050] Deglue at 120°C, let it stand for 14 hours to form a section of glue;
[0051] The second stage: use internal mixer, pass cooling water
[0...
Embodiment 2
[0068] The preparation technology of a kind of flexible nitrile double-sided adhesive fire hose described in the present embodiment comprises the following steps:
[0069] (1) Prepare raw materials:
[0070] Percentage by weight includes NBR / PVC7030: 53.6%, silica: 10%, plasticizer oil: 15%, activator: 2%, stearic acid: 0.8%, vulcanizing agent: 0.3%, accelerator: 1.3%, Calcium carbonate: 15%, methyl donor: 1.5%, methylene donor: 0.5%;
[0071] (2) Rubber mixing:
[0072] One stage: use internal mixer, pass cooling water,
[0073] Ingredients Temperature
[0074] NBR / PVC7030 70℃
[0075] Active agent + 1 / 3 white carbon black + 1 / 3 calcium carbonate + methyl donor 80°C
[0076] 1 / 3 white carbon black + 1 / 3 calcium carbonate + 1 / 2 plasticizer oil 95℃
[0077] 1 / 3 white carbon black + 1 / 3 calcium carbonate + 1 / 2 plasticizer oil 110℃
[0078] Deglue at 120°C, let it stand for 16 hours to form a section of glue;
[0079] The second stage: use internal mixer, pass cooling wat...
Embodiment 3
[0096] The preparation technology of a kind of flexible nitrile double-sided adhesive fire hose described in the present embodiment comprises the following steps:
[0097] (1) Prepare raw materials:
[0098] Percentage by weight includes NBR / PVC7030: 37.4%, silica: 25%, plasticizer oil: 5%, activator: 4%, stearic acid: 0.2%, vulcanizing agent: 0.7%, accelerator: 0.7%, Calcium carbonate: 25%, methyl donor: 0.5%, methylene donor: 1.5%;
[0099] (2) Rubber mixing:
[0100] One stage: use internal mixer, pass cooling water,
[0101] Ingredients Temperature
[0102] NBR / PVC7030 70℃
[0103] Active agent + 1 / 3 white carbon black + 1 / 3 calcium carbonate + methyl donor 80°C
[0104] 1 / 3 white carbon black + 1 / 3 calcium carbonate + 1 / 2 plasticizer oil 95℃
[0105] 1 / 3 white carbon black + 1 / 3 calcium carbonate + 1 / 2 plasticizer oil 110℃
[0106] Degumming at 120°C, standing for 12 hours to form a section of glue;
[0107] The second stage: use internal mixer, pass cooling water...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com