Preparation and application of novel environment-friendly foaming PVC specific uracil zinc composite stabilizer
A composite stabilizer, the technology of zinc uracil is applied in the field of preparation of a new type of environmental protection foamed PVC special uracil zinc composite stabilizer, which can solve the problems of production workers and the environment, high toxicity, poor thermal stabilization effect, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0033] Step 1, the preparation of zinc uracil;
[0034] Based on the quality of the total reactant, zinc uracil is prepared according to the following formula:
[0035] Uracil 100 parts
[0036] Phase transfer catalyst 2 parts
[0037] 520 parts of water
[0038] 260 parts of concentrated ammonia water
[0040] 210 parts of isopropanol
[0041] Add uracil and water into the 2L three-necked flask according to the above ratio, stir and heat to 50°C until the uracil is completely dissolved, then add concentrated ammonia water and phase transfer catalyst into the reaction kettle in sequence according to the above ratio, and after the dispersion is uniform, proceed Add zinc nitrate and isopropanol to this solution once, and continue to stir and react at this temperature for 2 h; The obtained product is dried in a vacuum oven, and finally dried and ground to obtain uracil zinc metal salt.
[0042] Step 2, compounding reaction;
[0043] Based o...
Embodiment 2
[0067] Step 1, the preparation of zinc uracil;
[0068] Based on the quality of the total reactant, zinc uracil is prepared according to the following formula:
[0069] Uracil 100 parts
[0070] 1.7 parts of phase transfer catalyst
[0071] 490 parts of water
[0072] 240 parts of concentrated ammonia water
[0074] 190 parts of isopropanol
[0075] Add uracil and water into the 2L three-necked flask according to the above ratio, stir and heat to 50°C until the uracil is completely dissolved, then add concentrated ammonia water and phase transfer catalyst into the reaction kettle in sequence according to the above ratio, and after the dispersion is uniform, proceed Add zinc nitrate and isopropanol to this solution for the second time, and continue to stir and react at this temperature for 2 h; after the reaction is completed, cool down to room temperature and take out the reaction mixture; Dry in a vacuum oven to obtain the product. Final...
Embodiment 3
[0101] Step 1, the preparation of zinc uracil;
[0102] Based on the quality of the total reactant, zinc uracil is prepared according to the following formula:
[0103] Uracil 100 parts
[0104] Phase transfer catalyst 1.5 parts
[0105] 460 parts of water
[0106] Concentrated ammonia water 220 parts
[0107] Zinc nitrate 120 parts
[0108] 170 parts of isopropanol
[0109] Add uracil and water into the 2L three-necked flask according to the above ratio, stir and heat to 50°C until the uracil is completely dissolved, then add concentrated ammonia water and phase transfer catalyst into the reaction kettle in sequence according to the above ratio, and after the dispersion is uniform, proceed Add zinc nitrate and isopropanol to this solution once, and continue to stir and react at this temperature for 2 h; The obtained product is dried in a vacuum oven, and finally dried and ground to obtain uracil zinc metal salt.
[0110] Step 2, compounding reaction;
[0111] Based on...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com