Method for producing weft-knitting suede fabric
A production method and technology of suede, applied in the directions of weft knitting, singeing, heating/cooling fabrics, etc., can solve the problems of high restriction, poor elasticity of suede, affecting the performance of fabrics, etc., to achieve less damage and feel Soft and good sanding effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] A kind of production method of weft-knitted suede, it comprises the following steps:
[0022] Step (1): weaving, weft knitting 20% T400 high elastic yarn and 80% sea-island yarn to form fabric, sea-island yarn is 90dtex / 36F sea-island yarn;
[0023] Step (2): Washing, putting the fabric in water at 50°C for washing;
[0024] Step (3): Open fiber, put the fabric into a solution containing caustic soda and M-1100 fiber opener, the bath ratio is 1:15, the temperature is 90°C, and the concentration of caustic soda is 2g / L;
[0025] Step (4): Singeing, passing the fabric quickly through the flame to burn off the fluff on the surface of the gray cloth, the flame temperature of singeing is 900°C;
[0026] Step (5): Dyeing, put the fabric and dye into the dyeing machine, the liquor ratio is 1:10, the dye includes dyeing agent, hydrogen peroxide, refining agent, chelating agent, basic dyeing auxiliaries;
[0027] Step (6): drying, drying the dyed fabric at a drying temperatu...
Embodiment 2
[0031] A kind of production method of weft-knitted suede, it comprises the following steps:
[0032] Step (1): weaving, weft knitting 26% T400 high elastic yarn and 74% sea-island yarn to form a fabric, and the sea-island yarn is 90dtex / 36F sea-island yarn;
[0033] Step (2): Washing, putting the fabric in water at 55°C for washing;
[0034] Step (3): Open fiber, put the fabric into a solution containing caustic soda and M-1100 fiber opener, the bath ratio is 1:20, the temperature is 92°C, and the concentration of caustic soda is 6g / L;
[0035] Step (4): Singeing, passing the fabric quickly through the flame to burn off the fluff on the surface of the gray cloth, the flame temperature of singeing is 1000°C;
[0036] Step (5): dyeing, put the fabric and dye into the dyeing machine, the liquor ratio is 1:12, the dye includes dyeing agent, hydrogen peroxide, refining agent, chelating agent, basic dyeing auxiliaries;
[0037] Step (6): drying, drying the dyed fabric at a drying ...
Embodiment 3
[0041] A kind of production method of weft-knitted suede, it comprises the following steps:
[0042] Step (1): weaving, 24% T400 high elastic yarn and 76% sea-island yarn are weft-knitted to form a fabric, and the sea-island yarn is 90dtex / 36F sea-island yarn;
[0043] Step (2): Washing, putting the fabric in water at 52°C for washing;
[0044] Step (3): Open fiber, put the fabric into a solution containing caustic soda and M-1100 fiber opener, the bath ratio is 1:18, the temperature is 92°C, and the concentration of caustic soda is 4.2g / L;
[0045] Step (4): singeing, passing the fabric through the flame quickly, burning off the fluff on the surface of the gray cloth, the flame temperature of singeing is 920°C;
[0046] Step (5): Dyeing, put the fabric and dye into the dyeing machine, the bath ratio is 1:11, the dye includes dyeing agent, hydrogen peroxide, refining agent, chelating agent, alkaline dyeing auxiliaries;
[0047] Step (6): drying, drying the dyed fabric at a d...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com