Organic rust conversion agent and preparation method and application method thereof
A transforming agent, rust technology, applied in the field of chemicals, can solve problems such as reducing the service life of equipment, and achieve the effect of prolonging the service life, using simple methods, and obtaining raw materials easily.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0017] Embodiment 1: An organic rust converting agent, comprising the following components in parts by weight: 8 parts of ethanol, 17 parts of tannic acid, 1 part of acetylacetone, 45 parts of phosphoric acid, 2 parts of methyl gallate, sodium benzenesulfonate 9 parts, water 12 parts. Wherein, the mass concentration of the ethanol is 35%. The mass concentration of the tannic acid is 55%. The mass concentration of the phosphoric acid is 25%.
[0018] When preparing the above-mentioned organic rust converting agent, proceed as follows:
[0019] 1) weigh according to the parts by weight of each component;
[0020] 2) Prepare sodium benzenesulfonate solution: mix and stir sodium benzenesulfonate and water to obtain sodium benzenesulfonate solution, set aside;
[0021] 3) Add ethanol into an open plastic bucket, then add tannin while stirring under the action of a stirrer, add acetylacetone to stir after the tannin is completely dissolved, and obtain a mixed solution when coole...
Embodiment 2
[0023] Embodiment 2: An organic rust conversion agent, comprising the following components in parts by weight: 5 parts of ethanol, 15 parts of tannic acid, 0.5 part of acetylacetone, 35 parts of phosphoric acid, 1 part of methyl gallate, sodium benzenesulfonate 8 parts, 10 parts water. Wherein, the mass concentration of the ethanol is 20%. The mass concentration of the tannic acid is 50%. The mass concentration of the phosphoric acid is 20%.
[0024] When preparing the above-mentioned organic rust converting agent, proceed as follows:
[0025] 1) weigh according to the parts by weight of each component;
[0026] 2) Prepare sodium benzenesulfonate solution: mix and stir sodium benzenesulfonate and water to obtain sodium benzenesulfonate solution, set aside;
[0027] 3) Add ethanol into an open plastic bucket, then add tannin while stirring under the action of a stirrer, add acetylacetone to stir after the tannin is completely dissolved, and obtain a mixed solution when cool...
Embodiment 3
[0029] Embodiment 3: An organic rust converting agent, comprising the following components in parts by weight: 10 parts of ethanol, 20 parts of tannic acid, 1.5 parts of acetylacetone, 65 parts of phosphoric acid, 3 parts of methyl gallate, sodium benzenesulfonate 10 parts, 18 parts of water. Wherein, the mass concentration of the ethanol is 60%. The mass concentration of the tannic acid is 60%. The mass concentration of the phosphoric acid is 30%.
[0030] When preparing the above-mentioned organic rust converting agent, proceed as follows:
[0031] 1) weigh according to the parts by weight of each component;
[0032] 2) Prepare sodium benzenesulfonate solution: mix and stir sodium benzenesulfonate and water to obtain sodium benzenesulfonate solution, set aside;
[0033] 3) Add ethanol into an open plastic bucket, then add tannin while stirring under the action of a stirrer, add acetylacetone to stir after the tannin is completely dissolved, and obtain a mixed solution wh...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com