Embodiment 1
[0031] This embodiment provides an anti-adhesive and viscosifying damping rubber, which is mainly formed by mixing raw materials. Wherein, the raw materials include: 35 parts by weight of asphalt, 10 parts by weight of softener, 20 parts by weight of heavy calcium and 35 parts by weight of tackifying resin.
[0032] The preparation method of the anti-adhesive and viscosifying damping adhesive includes: weighing the raw materials according to the above weight parts, and then mixing asphalt, softener, heavy calcium and tackifying resin and kneading at a temperature of 85° C. for 30 minutes.
Embodiment 2
[0034] This embodiment provides an anti-sticking and viscosifying damping rubber, which is mainly formed by mixing raw materials, wherein the raw materials include: 32 parts by weight of asphalt, 5 parts by weight of coumarone resin, 15 parts by weight of heavy calcium, and 32 parts by weight of tackifying resin. parts by weight.
[0035] The preparation method of the anti-adhesive and thickening damping adhesive comprises: weighing the raw materials according to the above weight parts, then mixing asphalt, coumarone resin, heavy calcium and tackifying resin and kneading for 40 minutes at a temperature of 80°C.
Embodiment 3
[0037] This embodiment provides an anti-adhesion and viscosity-increasing damping rubber, which is mainly formed by mixing raw materials. The raw materials include: 34 parts by weight of asphalt, 2 parts by weight of coumarone resin, 4 parts by weight of silicone oil, 18 parts by weight of talc powder and 34 parts by weight of viscose resin.
[0038] The preparation method of the anti-adhesive and thickening damping adhesive includes: weighing the raw materials according to the above weight parts, then mixing asphalt, coumarone resin, silicone oil, talcum powder and tackifying resin and kneading for 60 minutes at a temperature of 75°C .