Fluidized bed and process for covering flaky material in vapor phase method
A technology of sheet material and coating material, applied in the field of fluidized bed, can solve the problems of difficult ultra-fine sheet material, material sticking to the pipe wall, and poor coating quality, so as to improve coating efficiency and maintain pressure. drop, the effect of uniform gas distribution
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0055] Embodiment 1 A kind of U-type fluidized bed that is used for gas-phase method coating sheet material
[0056] A fluidized bed, the overall fluidized bed is U-shaped, which can be a pair of U-shaped or a combination of multiple pairs of U-shaped, and the cross-section of the U-shaped fluidized bed is circular, square, triangular, oval, One of the regular polygons; one upper port of the U-shaped fluidized bed is closed, and the other upper port is a switchable opening used as the feeding port 9; the two outer surfaces of the U-shaped fluidized bed are symmetrical A coating material inlet 5 is provided, and the coating material inlet 5 is 0.2 to 0.3 times the cross section of the U-shaped fluidized bed reaction chamber 3; the lower end of the U-shaped fluidized bed is provided with a fluidized gas inlet port 1;
[0057] The vertical reaction chamber 3 on both sides of the U-shaped fluidized bed is fixed with a gas distributor 4 whose maximum cross-sectional area is equal ...
Embodiment 2
[0060] Embodiment 2 utilizes the technique of the fluidized bed coating flake mica of embodiment 1
[0061] a. Take by weighing 450g average particle diameter of 30 μ m, diameter-thickness ratio is 31 flake mica (shape is conical or cylindrical), put the fluidized bed reactor through the detachable feeding port 9 at the upper end of the fluidized bed reactor In cavity 3;
[0062] b. Inject fluidizing gas nitrogen from fluidizing gas inlet 1, determine the flow rate through the pressure gauge, and adjust the fluidizing gas flow to 4.0m 3 / h, so that the flake mica is in suspension;
[0063] c. Adjust the temperature of the heating furnace body to 550°C, so that the reactor cavity 3 is at a stable temperature;
[0064] d. Liquid orthosilicate is sucked into the liquid vaporizer from the liquid storage tank through the liquid sampling pump, and after being vaporized at 170°C, it is passed into the fluidized bed reactor from the coating raw material inlet 5 at a speed of 1.0g / mi...