Surface coating device for aluminum profile, and method for coating the surface of aluminum profile with the device
A technology of surface coating and aluminum profiles, applied in the direction of surface reaction electrolytic coatings, coatings, electrolytic components, etc., can solve the problems of inability to recover the heat of the electrolyte, prolong the coating treatment cycle, and low heat utilization, and achieve shortening The effect of reducing processing time, shortening coating time, and improving automation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0054] Such as figure 1 As shown, the present invention discloses a surface coating device for aluminum profiles, comprising pickling tank 4, alkali washing tank 5, cleaning water tank 6 and oxidation tank 17 arranged in sequence, the pickling tank 4 is filled with dilute acid solution , the alkaline washing tank is filled with alkaline solution, the cleaning water tank 6 is filled with deionized water, the oxidation tank 17 is provided with an insulating sleeve 18, and there is a gap between the outer wall of the insulating sleeve 18 and the inner wall of the oxidation tank 17. gap, the gap is filled with cooling water, the insulating sleeve 18 is filled with electrolyte, the insulating sleeve 18 is hoisted with an electrode plate 22, and the electrode plate 22 is electrically connected to the electric control box 21 through a cathode wire.
[0055] In the cleaning water tank 6, a partition 61 is vertically arranged, and the partition 61 divides the inner chamber of the clean...
Embodiment 2
[0080] The present invention also discloses a method for coating an aluminum profile by using the above aluminum profile surface coating device, including the following steps:
[0081] (1) The aluminum profile is hoisted on the wire rope 24 of the electric hoist 3 through the coating bracket 23;
[0082] (2) Hang the aluminum profile into the left cleaning room, and completely submerge it in deionized water, start the ultrasonic generator 7, and clean for 3 to 5 minutes;
[0083] (3) Hang the aluminum profile into the pickling tank 4 and completely immerse it in the dilute acid solution. The residence time of the aluminum profile in the dilute acid solution is 2 to 4 minutes. The dilute acid solution includes dilute hydrochloric acid, dilute sulfuric acid, One or several kinds of dilute nitric acid;
[0084] (4) Hang the aluminum profile into the alkaline washing tank 5 and completely immerse it in the alkaline solution. The residence time of the aluminum profile in the alkal...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More 