A diatom mud coating and formaldehyde technology, applied in the direction of coating, can solve the problems of easy powder dropping, poor strength, and inability to degrade formaldehyde, etc., and achieve the effects of improving dispersion uniformity, simple preparation method and wide source of raw materials
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0030] A kind of preparation method of diatom mud coating that can degrade formaldehyde:
[0031] (1) Take 200 parts of low-grade diatomite, 40 parts of industrial waste acid, and 3 parts of sodium bicarbonate according to the mass ratio, and stir and mix;
[0032] (2) Roasting the mixed material obtained in step (1) at a temperature of 105° C. for 1 h;
[0033] (3) Disperse the calcined material obtained in step (2), add 4 parts of nano-titanium dioxide and 3 parts of cellulose ether, mix and stir thoroughly to obtain diatom mud coating.
Embodiment 2
[0035] A kind of preparation method of diatom mud coating that can degrade formaldehyde:
[0036] (1) Weigh 250 parts of low-grade diatomite, 60 parts of industrial waste acid, and 5 parts of sodium bicarbonate according to the mass ratio, and stir and mix;
[0037] (2) Roasting the mixed material obtained in step (1) at a temperature of 105° C. for 2 hours;
[0038] (3) After breaking up the calcined material obtained in step (2), add 4 parts of nano-titanium dioxide, 6 parts of cellulose ether, and 25 parts of colored sand and mix them thoroughly to obtain the diatom mud coating.
Embodiment 3
[0040] A kind of preparation method of diatom mud coating that can degrade formaldehyde:
[0041] (1) Weigh 180 parts of low-grade diatomite, 30 parts of industrial waste acid, and 4 parts of sodium bicarbonate according to the mass ratio, and stir and mix;
[0042] (2) Roasting the mixed material obtained in step (1) at a temperature of 110°C for 3h;
[0043] (3) After the calcined material obtained in step (2) is dispersed, add 2 parts of nano-titanium dioxide, 2 parts of cellulose ether, 40 parts of glass microspheres, 20 parts of seagull stone powder, 50 parts of paper-making white mud and mix fully, namely Get diatom mud coating.