Cast stone containing lubricating oil and preparation method thereof
A technology of lubricating oil and cast stone, applied in the field of lubricating oil containing cast stone and its preparation, to achieve the effects of cost reduction, strong adhesion and better dispersibility
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] A lubricating oil containing cast stone, comprising the following raw materials in parts by weight: 22 parts of mineral base oil, 17 parts of cast stone, 6 parts of modified zircon, 9 parts of dimethyl succinate, nonylphenol polyoxyethylene 4 parts of ether, 3 parts of polyvinyl alcohol, 6 parts of methyl carbamate, 7 parts of borate, 6 parts of triethylamine oleate, 7 parts of friction aid and 6 parts of surfactant.
[0031] A preparation method of lubricating oil containing cast stone, comprising the following preparation steps:
[0032] a. Put the cast stone into a ball mill for 5 hours, then place it at 800°C to melt, after cooling, add mineral base oil and polyvinyl alcohol, and carry out wet grinding for 2 hours. After the ball milling, use ultrasonic vibration to disperse for 10 minutes. Nanosuspension;
[0033] b. Introduce dimethyl succinate, methyl carbamate and nonylphenol polyoxyethylene ether into the reaction kettle, heat at 62°C until completely melted, ...
Embodiment 2
[0042] A lubricating oil containing cast stone, comprising the following raw materials in parts by weight: 18 parts of mineral base oil, 11 parts of cast stone, 7 parts of modified zircon, 5 parts of dimethyl succinate, nonylphenol polyoxyethylene 8 parts of ether, 7 parts of polyvinyl alcohol, 5 parts of methyl carbamate, 6 parts of borate, 8 parts of triethylamine oleate, 7 parts of friction aid and 3 parts of surfactant.
[0043] A preparation method of lubricating oil containing cast stone, comprising the following preparation steps:
[0044] a. Put the cast stone into a ball mill for 3 hours, then place it at 900°C to melt, after cooling, add mineral base oil and polyvinyl alcohol, and carry out wet milling for 2 hours. After the ball milling, use ultrasonic vibration to disperse for 15 minutes. Nanosuspension;
[0045] b. Introduce dimethyl succinate, methyl carbamate and nonylphenol polyoxyethylene ether into the reaction kettle, heat at 62°C until completely melted, t...
Embodiment 3
[0054] A lubricating oil containing cast stone, comprising the following raw materials in parts by weight: 21 parts of mineral base oil, 14 parts of cast stone, 8 parts of modified zircon, 7 parts of dimethyl succinate, nonylphenol polyoxyethylene 7 parts of ether, 5 parts of polyvinyl alcohol, 4 parts of methyl carbamate, 5 parts of borate, 9 parts of triethylamine oleate, 6 parts of friction aid and 4 parts of surfactant.
[0055] A preparation method of lubricating oil containing cast stone, comprising the following preparation steps:
[0056] a. Put the cast stone into a ball mill for 5 hours, and then melt it at 800°C. After cooling, add mineral base oil and polyvinyl alcohol, and carry out wet grinding for 2 hours. After the ball milling, use ultrasonic vibration to disperse for 15 minutes. Nanosuspension;
[0057] b. Introduce dimethyl succinate, methyl carbamate and nonylphenol polyoxyethylene ether into the reaction kettle, heat at 58°C until completely melted, then ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com