Yellowing-resistant and environment-friendly water-borne wood paint
A water-based wood lacquer and yellowing resistance technology, applied in the field of wood lacquer, can solve the problem that water-based wood lacquer has poor yellowing resistance, and achieve the effects of good dispersibility, increased service life and high transparency of the paint film
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] The invention is an anti-yellowing environmental protection water-based wood paint, which is prepared from the following raw materials in weight ratio:
[0016] Neopentyl glycol diethoxy diacrylate 24, sodium lauryl polyoxyethylene ether sulfate 2, polyether modified polydimethylsiloxane 3, talcum powder 2, nano-montmorillonite 1, cellulose hydroxyethyl Base ether 4, sodium dioctyl sulfosuccinate 7, polyoxyethylene cetyl stearyl diether 12, dihydroquinoline 3, amide wax emulsion 16, feldspar powder 4 and water 40.
[0017] Concrete preparation steps are as follows:
[0018] Each raw material component is added into a high-speed mixer according to the weight ratio, and after high-speed mixing for 40 minutes, the slurry released from the high-speed mixer is put into a colloid mill and circularly ground for 40 minutes to obtain the water-based wood varnish.
Embodiment 2
[0020] The invention is an anti-yellowing environmental protection water-based wood paint, which is prepared from the following raw materials in weight ratio:
[0021] Neopentyl glycol diethoxy diacrylate 35, sodium lauryl polyoxyethylene ether sulfate 8, polyether modified polydimethylsiloxane 6, talcum powder 4, nano-montmorillonite 3, cellulose hydroxyethyl Base ether 10, sodium dioctyl sulfosuccinate 3, polyoxyethylene cetyl stearyl diether 7, dihydroquinoline 1, amide wax emulsion 12, feldspar powder 1 and water 25.
[0022] Each raw material component is added into a high-speed mixer according to the weight ratio, and after high-speed mixing for 50 minutes, the slurry released from the high-speed mixer is put into a colloid mill and circulated for 30 minutes to obtain the water-based wood varnish.
Embodiment 3
[0024] A kind of anti-yellowing environmental protection water-based wood paint of the present invention is prepared from the raw materials of following weight ratio:
[0025] Neopentyl glycol diethoxy diacrylate 28, sodium lauryl polyoxyethylene ether sulfate 5, polyether modified polydimethylsiloxane 4, talcum powder 3, nano-montmorillonite 2, cellulose hydroxyethyl Base ether 8, sodium dioctyl sulfosuccinate 5, polyoxyethylene cetyl stearyl diether 11, dihydroquinoline 2, amide wax emulsion 14, feldspar powder 3 and water 30.
[0026] Concrete preparation steps are as follows:
[0027] Each raw material component is added into a high-speed mixer according to the weight ratio, and after high-speed mixing for 45 minutes, the slurry released from the high-speed mixer is put into a colloid mill and circulated for 35 minutes to obtain the water-based wood varnish.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com