Good-toughness plastic particle based on production of automobile parts and preparation method thereof
A technology of auto parts and plastic granules, applied in the field of plastic processing, can solve the problems of poor quality of finished products, insufficient comprehensive performance, uneven mixing and distribution of plastic materials, etc., and achieve long service life, excellent corrosion resistance and aging resistance, The effect of improving toughness
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0029] The raw materials include by weight: 70% of nylon material, 8% of toughening agent, 7% of short glass fiber, 5% of methyl phenyl vinyl silicone rubber, 5% of cis-1,4-polybutadiene rubber, Binder 2%, Toner 1.5% and Light Stabilizer 1.5%.
[0030] The invention also discloses a method for preparing plastic granules with good toughness for the production of auto parts, which specifically includes the following steps:
[0031] Step 1. Main material mixing: Take a certain amount of nylon material, methyl phenyl vinyl silicone rubber and cis-1,4-polybutadiene rubber, put them into a mixing mixer and preheat for 15 minutes;
[0032] Step 2. Primary melting: After the main materials are fully mixed, put the materials into the plastic extruder to heat and melt, and slowly add short glass fibers into the middle of the plastic extruder, so that the short glass fibers are evenly mixed into the molten plastic. Finally collect the completely molten material;
[0033] Step 3, mixing...
Embodiment 2
[0038] The raw materials include by weight: 75% of nylon material, 10% of toughening agent, 5% of short glass fiber, 3% of methyl phenyl vinyl silicone rubber, 2% of cis-1,4-polybutadiene rubber, Binder 3%, Toner 1% and Light Stabilizer 1%.
[0039] The invention also discloses a method for preparing plastic granules with good toughness for the production of auto parts, which specifically includes the following steps:
[0040] Step 1. Main material mixing: Take a certain amount of nylon material, methyl phenyl vinyl silicone rubber and cis-1,4-polybutadiene rubber, put them into a mixing mixer and preheat for 15 minutes;
[0041] Step 2. Primary melting: After the main materials are fully mixed, put the materials into the plastic extruder to heat and melt, and slowly add short glass fibers into the middle of the plastic extruder, so that the short glass fibers are evenly mixed into the molten plastic. Finally collect the completely molten material;
[0042] Step 3, mixing addi...
Embodiment 3
[0047] The raw materials include by weight: 80% nylon material, 10% toughening agent, 3% short glass fiber, 2% methyl phenyl vinyl silicone rubber, 2% cis-1,4-polybutadiene rubber, Binder 2%, Toner 0.5% and Light Stabilizer 0.5%.
[0048] The invention also discloses a method for preparing plastic granules with good toughness for the production of auto parts, which specifically includes the following steps:
[0049] Step 1. Main material mixing: Take a certain amount of nylon material, methyl phenyl vinyl silicone rubber and cis-1,4-polybutadiene rubber, put them into a mixing mixer and preheat for 15 minutes;
[0050] Step 2. Primary melting: After the main materials are fully mixed, put the materials into the plastic extruder to heat and melt, and slowly add short glass fibers into the middle of the plastic extruder, so that the short glass fibers are evenly mixed into the molten plastic. Finally collect the completely molten material;
[0051] Step 3, mixing additives: pu...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com