Heat insulation coating and production method thereof
A technology for thermal insulation coatings and production methods, which is applied in the field of architectural coatings, and can solve problems such as the influence of the sequence of raw material addition and different effects, and achieve the effects of good thermal insulation, convenient construction, and low volatility
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] A thermal insulation paint, which is composed of the following ingredients in weight percentage: 20% of water, 38% of perlite, 39% of acrylate emulsion, 2% of thickener, and the rest are pigments. Among them, the pigment is mainly used for coloring, adding more or less has no effect on the product.
[0017] The production method of the thermal insulation coating is as follows:
[0018] a. Take out the water according to the ratio, add acrylate emulsion, thickener, and sand powder to the water in sequence, and stir evenly while adding;
[0019] b. According to the color requirements of the product, add pigment and stir to mix;
[0020] c. Stir at high speed, adjust the speed of the mixer to make the speed reach 1500 rpm, and grind the fineness to 20-25um;
[0021] d. Scraper inspection to determine whether the fineness is up to standard.
[0022] The fineness of the final product is up to the standard, and the product grade is excellent; after testing, all indicators ...
Embodiment 2
[0024] A kind of thermal insulation paint, which is composed of the following components by weight: 21% water, 35% perlite, 40% acrylate emulsion, and 3% thickener. influences.
[0025] The production method of the thermal insulation coating is as follows:
[0026] a. Take out the water according to the ratio, add acrylate emulsion, thickener, and sand powder to the water in sequence, and stir evenly while adding;
[0027] b. According to the color requirements of the product, add pigment and stir to mix;
[0028] c. Stir at high speed, adjust the speed of the mixer to make the speed reach 1400 rpm, and grind the fineness to 20-25um;
[0029] d. Scraper inspection to determine whether the fineness is up to standard.
[0030] The fineness of the final product is up to the standard, and the product grade is excellent; after testing, all indicators of the product meet the requirements of coating production.
Embodiment 3
[0032] A kind of thermal insulation coating, which is composed of the following components by weight: 25% water, 37% perlite, 35% acrylate emulsion, and 3% thickener. influences.
[0033] The production method of the thermal insulation coating is as follows:
[0034] a. Take out the water according to the ratio, add acrylate emulsion, thickener, and sand powder to the water in sequence, and stir evenly while adding;
[0035] b. According to the color requirements of the product, add pigment and stir to mix;
[0036] c. Stir at high speed, adjust the speed of the mixer to make the speed reach 1300 rpm, and grind the fineness to 20-25um;
[0037] d. Scraper inspection to determine whether the fineness is up to standard.
[0038] The fineness of the final product is up to the standard, and the product grade is good; after testing, all indicators of the product meet the requirements of coating production.
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More