A resin anchoring agent and auxiliary device technology, which is applied in the installation of bolts, mining equipment, earthwork drilling and mining, etc., can solve the problems of high cost, poor heat resistance, low strength, etc., and achieve easy operation and safe construction technology Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0094] In addition, the present invention also provides a method for preparing a full-length anchoring resin anchoring agent, the preparation method comprising the following steps:
[0095] (1) Weigh the components required for the full-length anchoring resin anchoring agent according to the set ratio, and set aside;
[0096] (2) mix resin, accelerator, nano-SiO 2Stir and mix with the coupling agent at room temperature with a fast stirrer at a speed of more than 1200 rpm, disperse and stir for 30 to 40 minutes (for example, 31 minutes, 32 minutes, 33 minutes, 34 minutes, 35 minutes, 36 minutes, 37 minutes , 38 minutes, 39 minutes), to obtain the mixture after making it fully and evenly dispersed; the rotating speed of stirring and mixing in the fast stirrer is preferably 1200~2500 rev / min (such as 1300 rev / min, 1500 rev / min, 1800 rev / min , 2000 rpm, 2100 rpm, 2200 rpm, 2300 rpm, 2400 rpm, 2450 rpm).
[0097] (3) Next, mix the weighed stone powder with the mixture obtained in...
Embodiment 1
[0100] This embodiment provides a heat-resistant high-strength full-length anchoring resin anchoring agent. The heat-resistant high-strength full-length anchoring resin anchoring agent consists of the following raw material components in parts by weight:
[0101] 1) Mixed resin, 100 parts; Among them, 20 parts of PET type unsaturated polyester resin; 80 parts of novolac epoxy vinyl ester resin.
[0102] 2) stone powder, 500 parts; among them, coarse stone powder, 250 parts; fine stone powder, 250 parts.
[0103] 3) Accelerator, 1 part; Among them, DMA, 0.8 part; DMT, 0.2 part
[0104] 4) Nano SiO 2 , 1 copy;
[0105] 5) Additive, 0.5 part; wherein, the additive is KH-570 type silane coupling agent.
[0106] Weigh and measure all the raw material components of the heat-resistant high-strength full-length anchoring resin anchoring agent according to the ratio, and mix the PET type unsaturated polyester resin, phenolic epoxy vinyl ester resin, accelerator DMA, accelerator DMT,...
Embodiment 2
[0110] This embodiment provides a heat-resistant high-strength full-length anchoring resin anchoring agent. The heat-resistant high-strength full-length anchoring resin anchoring agent consists of the following raw material components in parts by weight:
[0111] 1) mixed resin, 100 parts; wherein, PET type unsaturated polyester resin, 30 parts; novolac epoxy vinyl ester resin, 70 parts.
[0112] 2) stone powder, 500 parts; among them, coarse stone powder, 250 parts; fine stone powder, 250 parts.
[0113] 3) Accelerator, 1 part; Among them, DMA, 0.7 part; DMT, 0.3 part
[0114] 4) Nano SiO 2 , 1 copy;
[0115] 5) Additive, 0.5 part; wherein, the additive is KH-570 type silane coupling agent.
[0116] Weigh and measure all the raw material components of the heat-resistant high-strength full-length anchoring resin anchoring agent according to the ratio, and mix the PET type unsaturated polyester resin, phenolic epoxy vinyl ester resin, accelerator DMA, accelerator DMT, nano-S...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com