Environment-friendly type polyurethane combined material and using method
A polyurethane composite material, an environmentally friendly technology, used in polyurea/polyurethane coatings, coatings, buildings, etc., can solve problems such as poor ventilation, harm to health, and small harm to human body.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] A component:
[0027] 330N: 27; Talc powder: 32; Calcium carbonate: 10; Silica: 2; Ethylene glycol: 3; TXIB: 20; Iron oxide red: 5;: 0.5; UV-9: 0.5; Bismuth octoate): 2.0
[0028] During preparation, polyether polyol 330N, filler (talc powder, calcium carbonate, white carbon black), crosslinking agent ethylene glycol, plasticizer TXIB, pigment iron oxide red, antiaging agent BHT, ultraviolet absorber UV- 9 Add it to the reaction kettle and stir evenly, then add it to a colloid mill or a three-roller grinder to grind until the fineness is below 80um, then vacuumize and dehydrate and degas at 80°C-100°C for 2-3 hours, then cool down to 40°C Add the organic bismuth catalyst, stir evenly, and pack into barrels.
[0029] B component:
[0030] DL-3000: 48; Pure MDI: 52
[0031] Preparation: Add polyether polyol to the reaction kettle at room temperature, stir at 80°C-100°C, vacuumize and dehydrate for 2-3 hours, cool down to 40°C, add diphenylmethane diisocyanate, 80-85°C...
Embodiment 2
[0034] A component:
[0035] MN-3050: 40; Talcum powder: 25; Clay: 9; Silica: 2; Butanediol: 2; TXIB: 15; Iron oxide red: 5; 1010: 1; UV531: 1; Bismuth alkanoate): 1.0
[0036] B component:
[0037] DL-2000: 68; Pure MDI: 32
[0038] During on-site construction, according to the weight ratio of component A: component B = 2:1, mix well, lay and cure.
Embodiment 3
[0040] MN-3050: 40; DL-2000: 20; Talc powder: 17; Silica: 2; Propylene glycol: 5; TXIB: 10; Iron yellow: 5; BHT: 0.5; Bismuth quinanoate): 5.0
[0041] B component:
[0042] DL-3000: 80; Pure MDI: 20
[0043] During on-site construction, according to the weight ratio of component A: component B = 5:1, mix well, lay and cure.
PUM
Property | Measurement | Unit |
---|---|---|
elastic recovery rate | aaaaa | aaaaa |
elongation at break | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com