Water-soluble water-resistant printing ink for plastic woven sack and preparation thereof
A plastic woven bag and water-soluble technology, which is applied in the field of water-soluble and water-resistant plastic woven bag ink and its preparation, can solve the problems of solvents that harm human health, affect food safety, and low water resistance level, and achieve good printing adaptability and safety Good performance and safe use
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] Raw materials: 50% acrylic acid added rosin resin, 10% N330 carbon black, 14% water, 9% ammonia water, 11% J624 emulsion, 4.5% water-based wax, 1% leveling agent, 0.5% defoamer according to the formula , the above percentages are mass percentages.
[0027] Preparation process of water-soluble water-resistant plastic woven bag surface printing black ink:
[0028] a) Take acrylic acid-added rosin resin according to the formula, add ammonia water to make it aminated to achieve water solubility; the pH of the solution after amination is 8.5.
[0029] b) Put the non-toxic pigment, water, pure acrylic emulsion and above-mentioned resin after amination into the dispersing tank according to the formula, fully stir and disperse evenly;
[0030] c) Move the dispersed materials to a sand mill and grind them for 3 to 4 times until the measured fineness reaches below 20 μm, otherwise continue grinding until the fineness meets the requirements;
[0031] d) After the ground material...
Embodiment 2
[0036] Take 55% acrylic acid added rosin resin, 8% 198 Lithol scarlet, 12% water, 8% ammonia water, 10% J624 emulsion, 5% water-based wax, 1% leveling agent, 0.5% defoamer according to the formula, The above percentages are all percentages by mass. According to the operation steps of Example 1, the water-soluble water-resistant plastic woven bag composite red ink can be prepared, and its main technical indicators are shown in Table 2:
[0037] Table 2
[0038] project
Embodiment 3
[0040] According to the formula, take 50% acrylic acid addition rosin resin, 6.5% phthalocyanine blue, 1.5% titanium dioxide, 13% water, 10% ammonia water, 10% J624 emulsion, 5% water-based wax, 1% leveling agent, 0.5% defoaming agent agent, the above percentages are mass percentages. According to the operation steps of Example 1, the water-soluble and water-resistant plastic woven bag composite blue ink can be prepared, and its main technical indicators are shown in Table 3:
[0041] table 3
[0042] project
[0043] The acrylic acid addition rosin resin of above-described embodiment is available in the market, and the manufacturer is Wuhan Lisheng Chemical Raw Material Research Institute; Ammonia is available in the market, and the concentration is 28% (percentage by weight) and the manufacturer is Wuhan Ammonia Factory; J624 emulsion is It is available in the market, and the manufacturer is Taiwan Johnson Polymer Chemical Co., Ltd.; the water-based wax is availa...
PUM
Property | Measurement | Unit |
---|---|---|
Fineness | aaaaa | aaaaa |
Freshness | aaaaa | aaaaa |
Freshness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com