Filter media and preparation method, filter element, purifier and drinking machine using the filter media
A filter medium and filter element technology, applied in beverage preparation devices, filtration separation, separation methods, etc., can solve the problems of complex treatment process, low efficiency, poor effect, etc., and achieve the effect of improving water quality, simple method and low cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0035] (1) Take 220 grams of ultra-high molecular weight polyethylene powder, said ultra-high molecular weight polyethylene is the M-III type product of Beijing Dongfang Petrochemical Co., Ltd. Auxiliary No. 2 Factory, and its molecular weight is 3.5 million;
[0036] (2) Take by weighing 180 grams of medical activated carbon powder, the particle diameter of the medical activated carbon is 38~250 microns;
[0037] (3) Take by weighing 80 grams of sepiolite powder, the particle diameter of the sepiolite powder is 18~150 microns, the sepiolite powder is through acidification and activation treatment, and the concrete acidification treatment process is: using concentration is 10% sulfuric acid at temperature Soak at 60°C for 12h, then wash with deionized water, and bake at 300°C for 3h;
[0038] (4) Take by weighing 60 grams of natural clinoptilolite powder, the particle size of which is 44-124 microns, the natural clinoptilolite powder is treated by acidification and activation,...
Embodiment 2
[0044] (1) Take 150 grams of ultra-high molecular weight polyethylene powder, said ultra-high molecular weight polyethylene is the M-III type product of Beijing Dongfang Petrochemical Co., Ltd. Auxiliary No. 2 Factory, and its molecular weight is 3.5 million;
[0045] (2) Take by weighing 140 grams of medical activated carbon powder, the particle diameter of the medical activated carbon is 178~250 microns;
[0046] (3) Take 70 grams of sepiolite powder, the particle diameter of the sepiolite powder is 38~150 microns, and the sepiolite powder is processed through acidification and activation. Soak at 60°C for 12h, then wash with deionized water, and bake at 300°C for 3h;
[0047] (4) Weigh 65 grams of natural clinoptilolite powder, the particle diameter of which is 44-124 microns, the natural clinoptilolite powder is processed through acidification and activation, and the specific treatment acidification process is: use HCl Soak with NaCl mixed solution for 6 hours, where the ...
Embodiment 3
[0051] (1) Take 180 grams of ultra-high molecular weight polyethylene powder, said ultra-high molecular weight polyethylene is the M-II type product of Beijing Dongfang Petrochemical Co., Ltd. Auxiliary No. 2 Factory, and its molecular weight is 2.5 million;
[0052] (2) Take by weighing 170 grams of medical activated carbon powder, the particle diameter of the medical activated carbon is 89~178 microns;
[0053] (3) Take by weighing 60 grams of sepiolite powder, the particle diameter of the sepiolite powder is 38~178 micron, this sepiolite powder is through acidification and activation treatment, and concrete acidification treatment process is: use the sulfuric acid that concentration is 10% at temperature Soak at 60°C for 12h, then wash with deionized water, and bake at 300°C for 3h;
[0054] (4) Weigh 80 grams of natural clinoptilolite powder, the particle diameter of which is 44 to 124 microns. The natural clinoptilolite powder is subjected to acidification and activation ...
PUM
| Property | Measurement | Unit |
|---|---|---|
| particle diameter | aaaaa | aaaaa |
| particle diameter | aaaaa | aaaaa |
| specific surface area | aaaaa | aaaaa |