A technology for titanium-rich material and titanium concentrate, applied in the field of metallurgy, can solve the problems of complex operation, large grade fluctuation, and corrosion of furnace lining production, and achieve the effects of easy operation, stable reduction degree, and stable control of process parameters.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] Make ingredients according to Table 1, and mix evenly.
[0029] Table 1 Pellet ingredient list
[0030] Serial number
raw material name
Granularity / mm
Ratio / %
1
Titanium Concentrate
≤0.088
75
2
≤0.1
19
3
Sodium borate
≤0.1
3
4
≤0.1
2
5
≤0.1
1
6
Water (additional)
7
[0031] The material is compressed into 15mm pellets, and the pellets are put into a special refractory tank and put into a tunnel kiln for reduction. The reduction temperature of the tunnel kiln is controlled at 1130℃ and the reduction time is controlled at 120min.
[0032] After the pellets are naturally cooled, they are finely ground in a ball mill. After magnetic separation, iron powder and titanium-rich material are separated. The recovery rate of iron powder is 91%, the grade of titanium dioxide in the titanium-rich material is 78%, and the recovery rate of titanium is up to 93%.
[0033] The separated titanium-rich ma...
Embodiment 2
[0035] Make ingredients according to Table 2 and mix evenly.
[0036] Table 2 Pellet ingredient list
[0037] Serial number
raw material name
Granularity / mm
Ratio / %
1
Titanium Concentrate
≤0.088
77
2
≤0.1
17
3
Sodium borate
≤0.1
2
4
≤0.1
2
5
≤0.1
2
6
Water (additional)
7
[0038] The material is compressed into 18mm pellets, and the pellets are put into a special refractory tank and put into a tunnel kiln for reduction. The reduction temperature of the tunnel kiln is controlled at 1150℃ and the reduction time is controlled at 110min.
[0039] After the pellets are naturally cooled, they are finely ground in a ball mill. After magnetic separation, iron powder and titanium-rich material are separated. The recovery rate of iron powder is 92%, the grade of titanium in the titanium-rich material is 77%, and the recovery rate of titanium is up to 91%.
[0040] The separated titanium-rich material is...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com