A filling material and entry retaining technology, which is applied in the field of paste pumping filling materials and preparations for mine entry retaining support, can solve problems such as unfavorable market promotion, waste of energy costs, and environmental pollution, so as to reduce production costs and improve mine safety. Production security and pollution reduction effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] Natural anhydrite 15%-18%
[0028] Cement 15%-20%
[0029] Fly ash or blast furnace slag 18%-25%
[0030] Air-entraining agent 0.03%-0.08%
[0031] Stimulator 0.5%-1.0%
[0032] Early strength agent 1.5-2.5%
[0033] Accelerator 0.6%-0.8%
[0034] Water reducing agent 0.5%-0.8%
[0035] Pebbles 20%-25%
[0036] River sand 20%-25%
[0037] During preparation, the natural anhydrous gypsum is first ground by an industrial ball mill, the fineness is controlled at 200 mesh sieve, the balance is less than 1%, and the specific surface area is 4000-5000cm 2 / g; After fully mixing the air-entraining agent, activator, accelerator, early strength agent, and water reducer in a given proportion, mix it with river sand, stones, anhydrite powder, cement and fly ash in a given proportion Mix evenly in the mixer to form a paste pumping filling material for mine roadway retaining support, and then pack it into a product. The paste pumping filling material obtained in this embodi...
Embodiment 2
[0039] Natural anhydrite 2%-3%
[0040] Cement 15%-25%
[0041] Fly ash or slag 18%-25%
[0042] Air-entraining agent 0.01%-0.04%
[0043] Stimulator 0.5%-1.0%
[0044] Early strength agent 0.5-1.5%
[0045] Accelerator 0.8%-1.2%
[0046] Water reducing agent 0.5%-0.8%
[0047] Pebbles 20%-25%
[0048] River sand 20%-25%
[0049] During preparation, the natural anhydrous gypsum is first ground by an industrial ball mill, the fineness is controlled at 200 mesh sieve, the balance is less than 1%, and the specific surface area is 4000-5000cm 2 / g; After fully mixing the air-entraining agent, activator, accelerator, early strength agent, and water reducer in a given proportion, mix it with river sand, stones, anhydrite powder, cement and fly ash in a given proportion Mix evenly in the mixer to form a paste pumping filling material for mine roadway retaining support, and then pack it into a product. The paste pumping filling material obtained in this embodiment has good fl...
Embodiment 3
[0051] Natural anhydrite 10%-15%
[0052]Cement 15%-20%
[0054] Air-entraining agent 0.03%-0.08%
[0055] Stimulator 0.5%-1.0%
[0056] Early strength agent 1.0-1.5%
[0057] Accelerator 0.3%-0.6%
[0058] Water reducing agent 0.6%-1.0%
[0059] Pebbles 20%-25%
[0060] River sand 20%-25%
[0061] During preparation, the natural anhydrous gypsum is first ground with an industrial ball mill, the fineness is controlled at 200 mesh sieve, the balance is less than 1%, and the specific surface area is 4000-5000cm 2 / g; After fully mixing the air-entraining agent, activator, accelerator, early strength agent, and water reducer in a given proportion, mix it with river sand, stones, anhydrite powder, cement and fly ash in a given proportion Mix evenly in the mixer to form a paste pumping filling material for mine roadway retaining support, and then pack it into a product. The paste pumping filling material for mine roadway retaining support obta...
PUM
Property | Measurement | Unit |
---|---|---|
specific surface area | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com