Water-based woven bag ink and preparation method thereof
A woven bag and ink technology, which is applied in the field of printing ink, can solve the problems of woven bag ink that cannot meet the needs of the market, air pollution in printing workshops, and insufficient endurance, so as to improve the overall environmental quality, reduce fire hazards, and Good scraping effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment approach 1
[0020] According to the molar ratio of rosin: maleic anhydride: TDI: pentaerythritol = 18:9.5:2.9:3.3, first heat and melt the rosin, then heat the maleic anhydride at 175-180°C for 0.9 hours, add TDI (toluene diisocyanate) for 1 hour, Add pentaerythritol and raise the temperature to 230°C for 1.8 hours. Then water, ammoniacal liquor and the water-soluble resin of making are dissolved into 38% solid content resin liquid; Get the weight percent of component again and be water-based resin liquid 69%, pigment 8%, defoamer 1%, micropowder wax 1.6% % to 2.4%, plasticizer 1.2%, erucamide 1.2%, water 18% to prepare water-based woven bag ink.
Embodiment approach 2
[0022] According to the molar ratio of rosin: maleic anhydride: TDI: pentaerythritol = 20: 9.5: 3.1: 3.2, first heat and melt the rosin, then heat the maleic anhydride at 185-190°C for 1 hour, add TDI (toluene diisocyanate) for 1 hour, Add pentaerythritol and raise the temperature to 240°C for 2 hours. Then water, ammoniacal liquor and the water-soluble resin of making are dissolved into 39% solid content resin liquid; Get the percentage by weight of component again and be water-based resin liquid 70%, pigment 9%, defoamer 1.1%, micropowder wax 2 %, plasticizer 1.2%, erucamide 1.2%, water 15.5% to prepare water-based woven bag ink.
Embodiment approach 3
[0024] According to the molar ratio of rosin: maleic anhydride: TDI: pentaerythritol = 20:10:3:3, first heat and melt the rosin, then heat the maleic anhydride at 180-185°C for 1 hour, add TDI (toluene diisocyanate) for 1 hour, Add pentaerythritol and raise the temperature to 240°C for 2 hours. Then water, ammoniacal liquor and the water-soluble resin of making are dissolved into 35% solid content resin liquid; The percentage by weight of getting component is water-based resin liquid 75%, pigment 10%, defoamer 1%, micropowder wax 2 %, 1% plasticizer, 1% erucamide, and 10% water to prepare water-based woven bag ink.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com