Method for preparing high-intensity water-resistant multifunctional high-efficient granule active clay preparation and use thereof
A technology of activated clay and water resistance, used in chemical instruments and methods, other chemical processes, alkali metal oxides/hydroxides, etc., to improve oil quality and deodorization ability, broad market prospects, and improve product quality. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0042] The preparation method of granular activated clay preparation comprises the following steps:
[0043] 1) Select 1 ton of bentonite raw ore to be crushed by rough rolling, and then put 1.2 tons of water into the slurry tank for stirring to make slurry with a certain specific gravity;
[0044]2) Stir the slurry for 2 hours to make the specific gravity reach 1.2 tons / m 3 ;
[0045] 3) Add 200KG concentrated sulfuric acid with a concentration of 98% to the slurry in the activation kettle, feed steam and stir to heat up to 90°C, keep the temperature for 5 hours, then cool and discharge to the rinsing tank to remove the larger specific gravity at the bottom of the slurry Sand and gravel impurities (conventional process method);
[0046] 4) Stir while adding water in the rinsing tank, stir for 1.5 hours, stand still for 2 hours, put the upper layer of acid solution into the waste acid tank (as the next batch of slurry for acid preparation), add water for the second rinse and...
Embodiment 2
[0053] The preparation method of granular activated clay preparation comprises the following steps:
[0054] 1) select 1 ton of bentonite raw ore to be crushed by rough rolling, and put into 1.3 tons of water slurry tank for stirring to make slurry with a certain specific gravity;
[0055] 2) Stir the slurry for 2.5 hours to make the specific gravity reach 1.35 tons / m 3 ;
[0056] 3) Adding 350KG concentration to the slurry is 98% concentrated sulfuric acid, heat preservation reaction at a temperature of 105° C. for 6 hours, then cool and discharge to the rinsing tank to remove sandstone and impurities with larger proportion in the slurry.
[0057] 4) Stir while adding water in the rinsing tank, stir for 1 hour, stand still for 1.5 hours, put the upper layer of acid solution into the waste acid tank (as the next batch of slurry for acid preparation), add water for the second time and then repeat the previous The process requires about 3-4 times of repeated rinsing, and the a...
Embodiment 3
[0064] The preparation method of granular activated clay preparation comprises the following steps:
[0065] 1) Select 1 ton of bentonite raw ore to be crushed by rough rolling, then add 1.4 tons of water to the pulping tank for stirring to make a slurry with a certain specific gravity;
[0066] 2) Stir the slurry for 3 hours to make the specific gravity reach 1.4 tons / m 3 ;
[0067] 3) Add 450KG concentration of 98% concentrated sulfuric acid to the slurry, heat up to 100°C and keep warm for 6.5 hours, then cool and discharge to the rinsing tank to remove sandstone and impurities with larger proportion in the slurry;
[0068] 4) Stir while adding water in the rinsing tank, stir for 2 hours, stand still for 2.5 hours, put the upper layer of acid solution into the waste acid tank (as the next batch of slurry for acid preparation), add water for the second time and then repeat the previous The process requires about 3-4 times of repeated rinsing, and the water consumption for ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com