A technology for limestone and ore bricks, applied in the field of bricks and preparation, can solve the problems of serious stockpiling and low utilization rate of limestone tailings, and achieve the effects of solving the problem of land resources, expanding the source of raw materials and low production cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] A limestone tailings brick, its components and weight percentages are: limestone tailings: 92%, sand solidifying agent: 8%.
[0023] Preparation steps:
[0024] 1) The limestone tailings are dehydrated by natural air drying or heat drying, so that the water content of the limestone tailings is 14.5%;
[0025] 2) Continue to take natural air drying or heat drying to carry out dehydration treatment, so that the water content of the limestone tailings is 4.5%;
[0026] 3) Use sieves for sorting, and remove lumps with a particle size of ≥5 mm; limestone tailings with a particle size of ≥5 mm are rolled to a particle size of ≤5 mm before use (the same below);
[0027] 4) Stir and mix with a mixer, and the mud content after mixing is controlled to be 20% of the total weight;
[0028] 5) uniformly mixing 92% limestone tailings with a particle size of ≤5 mm and 8% sand curing agent by weight;
[0029] 6) Add water and stir until uniform, the water content of the mixed raw ma...
Embodiment 2
[0032] A limestone tailings brick has the following components and weight percentages: limestone tailings: 70%, HAS curing agent: 9%, fly ash 21%.
[0033] Preparation steps:
[0034] 1) The limestone tailings are dehydrated by natural air drying or heat drying, so that the water content of the limestone tailings is 12.5%;
[0035] 2) continue to take natural air drying or heat drying for dehydration treatment, so that the water content of the limestone tailings is 3.0%;
[0036] 3) Use a sieve to sort, and remove lumps with a particle size ≥ 5 mm;
[0037] 4) Stir and mix with a mixer, and the mud content after mixing is controlled to be 20% of the total weight;
[0038] 5) uniformly mixing 70% limestone tailings, 9% HAS curing agent and 21% fly ash with a particle size of ≤5 mm;
[0039] 6) Add water and stir until uniform, the water content of the mixed raw materials is 8.0% by weight;
[0040] 7) Carry out brick making and maintenance.
Embodiment 3
[0042] A limestone tailings brick, its components and weight percentages are: limestone tailings: 60.0%, HEC consolidation agent: 10%, sandstone coarse aggregate 30%.
[0043] Preparation steps:
[0044] 1) The limestone tailings are dehydrated by natural air drying or heat drying, so that the water content of the limestone tailings is 12.5%;
[0045] 2) continue to take natural air-drying or heat-drying to carry out dehydration treatment, make the water content of limestone tailings be 3.6%;
[0046] 3) Use a sieve to sort, and remove lumps with a particle size ≥ 5 mm;
[0047] 4) Stir and mix with a mixer, and the mud content after mixing is controlled to be 20% of the total weight;
[0048] 5) uniformly mixing 60% limestone tailings, 10% HEC consolidating agent and 30% sand-stone phase aggregate with a particle size of ≤5 mm;
[0049] 6) Add water and stir until uniform, the water content of the mixed raw materials is 6.5% by weight;
[0050] 7) Carry out brick making a...
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com