Aqueous anti-doodling paint and preparation method thereof
An anti-graffiti and coating technology, applied in the field of coatings, to achieve the effects of enhanced interaction, anti-penetration pollutant adhesion, and high density
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0073] The preparation method of water-based anti-graffiti coating includes steps such as premixing, grinding and dispersing, adding emulsion and adding additives, and its specific process steps are as follows:
[0074] (1). Pre-mixing: Add the above-mentioned parts by weight of water, dispersant, defoamer and wetting agent into the dispersing tank, stir and mix well to facilitate the dispersion of fillers. The stirring speed is controlled at 300-500RPM.
[0075] (2). Grinding and dispersing: Add the above-mentioned glass powder in parts by weight, beating and grinding for 15-20 minutes under high-speed dispersion, so that the fineness of the color paste is qualified when it is below 50um, and the filler particles are stirred at a high shear rate at high speed. Under the action, it is dispersed into primary particles, and a stable state of dispersion is obtained under the action of the dispersing aid system. The speed of beating and grinding is controlled at 1500-2000RPM.
[0...
Embodiment 1
[0083] The parts by weight of water-based anti-graffiti paint are as follows:
[0084] water 8
[0085] GA40 (dispersant) 0.1
[0086] TEXONAL (coalescent aid) 1
[0087] CF10 (wetting agent) 0.05
[0088] CF245 (defoamer) 0.2
[0089] glass powder 15
[0090] M8 (mold inhibitor) 0.15
[0091] LXE (preservative) 0.15
[0092] DIRTSHIELD K2 (Pure Acrylic Emulsion) 60
[0093] TT935 (thickener) 1.2
[0094] Ethylene glycol 1.5
[0095] FSE (fluorine additive) 0.05
[0096] HF200 (wax emulsion) 0.6.
[0097] The preparation process of the preparation method of the above-mentioned water-based anti-graffiti coating includes steps such as premixing, grinding and dispersing, adding emulsion and auxiliary agents, and the specific process steps are as follows:
[0098] (1). Pre-mixing: Add the above-mentioned parts by weight of water, GA40 (dispersant), CF245 (defoamer) and CF10 (wetting agent) into the dispersion tank, and make it fully mixed evenly, so as to facilitate t...
Embodiment 2
[0106] The parts by weight of water-based anti-graffiti paint are as follows:
[0107] water 5
[0108] GA40 (dispersant) 0.15
[0109] TEXONAL (film-forming aid) 1.2
[0110] CF10 (wetting agent) 0.1
[0111] CF245 (defoamer) 0.2
[0112] glass powder 18
[0113]M8 (mold inhibitor) 0.15
[0114] LXE (preservative) 0.15
[0115] DIRTSHIELD K2 (Pure Acrylic Emulsion) 65
[0116] TT935 (thickener) 1
[0117] Ethylene glycol 1.5
[0118] FSE (fluorine additive) 0.08
[0119] HF200 (wax emulsion) 0.5.
[0120] The preparation process of the preparation method of the above-mentioned water-based anti-graffiti coating includes steps such as premixing, grinding and dispersing, adding emulsion and auxiliary agents, and the specific process steps are as follows:
[0121] (1). Pre-mixing: Add the above-mentioned parts by weight of water, GA40 (dispersant), CF245 (defoamer) and CF10 (wetting agent) into the dispersion tank, and make it fully mixed evenly, so as to facilitate ...
PUM
Property | Measurement | Unit |
---|---|---|
Drying time | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com