Preparation method of modified casein for leather finishing
A modified technology of casein, which is applied in leather surface treatment, small raw hide/big raw hide/leather/fur treatment, small raw hide/large raw hide/leather skin/fur chemical treatment, etc. It can solve the problem of poor surface adhesion, No problems such as extensibility, cold brittleness and hot stickiness, etc., to achieve the effect of strong adhesion, good water resistance, and hard film formation
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2011-05-04
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
[0001] Technical field
[0002] The invention relates to a preparation method of modified casein for leather finishing. Background technique
[0003] In order to ensure the natural performance of leather products and have a comfortable feel and aesthetic feeling, leather finishing agents are often used to achieve the above-mentioned purposes in the process of leather production and processing. The cream casein coating material plays an important role in surface coating. Casein coating materials have the advantages of bright coating, high temperature ironing resistance and suitable for polishing. Sticky and other shortcomings. Contents of the invention
[0004] In order to solve the above problems, the present invention proposes a preparation method of modified casein for leather finishing.
[0005] In order to ensure that the effect designed by the present invention is achieved and it is convenient to use, the preparation method of the GR-modified casein of the present in...
Examples
Embodiment Construction
[0026] (1) Take the following raw materials according to the process ratio:
[0027] Boiling Water, Casein, Ammonia (18%), TX-10, Sage Oil (70%), Ethylene Glycol, Ammonium Persulfate, Ammonium Caprolactam, Phenol, Sodium Benzoate, Glycerin.
[0028] (2) Add 85% of the total amount of boiling water in the formula into the reactor, and then add the amount of ammonia in the formula, then start stirring;
[0029] (3) Add the casein of formula quantity and heat and stir until all dissolve;
[0030] (4) Add the TX-10 of formula quantity and stir for half an hour;
[0031] (5) Add the Taikoo oil of formula quantity and stir for 1 hour;
[0032] (6) Cool the boiling water with 4.8% of the total amount of the formula to 50-60° C., add caprolactam with 37.5% of the total amount of the formula, and make it all dissolve for later use;
[0033] (7) Cool the boiling water with 8.9% of the total amount of the formula to 50-60° C., add caprolactam ammonium with 62.5% of the total amount of...