Reactive polymer cement waterproof coating
A waterproof coating and polymer technology, used in polyurea/polyurethane coatings, coatings, etc., can solve the problems of long construction period, poor water resistance, and inability to dry and solidify, and achieves low construction environment requirements, excellent mechanical properties, and excellent waterproof. performance effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] Preparation of organic components: Add 1129g of polyether diol, 756g of polyether triol, and 586g of plasticizer into a 5L four-necked reaction flask, heat up to 100°C-120°C for vacuum dehydration for 4 hours, and cool down below 50°C. Add 290g of toluene diisocyanate, heat up slowly, control the temperature at 80-85°C, react under vacuum for 2.5h, cool down at 50-60°C, add 2g of defoamer (E-7), 1.5g of catalyst dibutyltin dilaurate (T-12) Stir for 1 hour, seal the discharge to obtain the organic component.
[0020] Preparation of the inorganic component: 500g of cement and 500g of quartz powder were mixed and dispersed evenly to obtain the inorganic component.
[0021] The weight ratio of each component: organic component: inorganic component: water=1:1:0.6
Embodiment 2
[0023] The preparation of the organic components follows Example 1.
[0024] Preparation of the inorganic component: 500g of cement and 1000g of quartz powder were mixed and dispersed evenly to obtain the inorganic component.
[0025] The weight ratio of each component: organic component: inorganic component: water=1:1:0.6
Embodiment 3
[0027] Preparation of organic components: Add 1129g of polyether diol, 756g of polyether triol, and 586g of plasticizer into a 5L four-necked reaction flask, heat up to 100°C-120°C for vacuum dehydration for 4 hours, and cool down below 50°C. Add 417g of diphenylmethane diisocyanate, heat up slowly, control the temperature at 80-85°C, react under vacuum for 2.5h, lower the temperature at 50-60°C, add 2g of defoamer (E-7), 1.5g of catalyst dilaurel Acid dibutyltin (T-12) was stirred for 1 hour, and the discharge was sealed to obtain the organic component.
[0028] Preparation of the inorganic component: 500g of cement and 500g of quartz powder were mixed and dispersed evenly to obtain the inorganic component.
[0029] The weight ratio of each component: organic component: inorganic component: water=1:1:0.6
PUM
Property | Measurement | Unit |
---|---|---|
hydroxyl value | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com