Ink for soft package intaglio printing and preparation method thereof
A technology of gravure printing and flexible packaging, applied in the field of gravure printing ink for flexible packaging and its preparation process, can solve the problems of poor color reproducibility, poor application tolerance, and ink not suitable for high magnetic environments, etc., and achieve superior refreezing performance and transfer Excellent performance and good color reproducibility
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] 1) Put in 25 parts of acrylic resin and 30 parts of water; start the machine to stir, and put in 38 parts of pigment during the stirring process;
[0020] 2) After stirring for 20 minutes, add 2 parts of dispersant and 5 parts of defoamer, grind for 3 hours, and filter the material with a 2 μm filter to obtain the color paste;
[0021] 3) Add 50 parts of water-based acrylic emulsion, 20 parts of water, and 25 parts of color paste in sequence, and stir and mix evenly;
[0022] 4) Add 3 parts of 1.2-benzisothiazolin-3-one and stir for 15 minutes;
[0023] 5) Add 2 parts of hardness polyethylene emulsion and stir for 5 minutes, filter and pack.
Embodiment 2
[0025] 1) Put in 23 parts of acrylic resin and 30 parts of water, start the machine to stir, and put in 40 parts of pigment during the stirring process;
[0026] 2) After stirring for 20 minutes, add 2 parts of dispersant and 5 parts of defoamer, grind for 3 hours, and filter the material with a 2 μm filter to obtain a color paste.
[0027] 3) Add 50 parts of water-based acrylic emulsion, 21 parts of water, and 25 parts of color paste in sequence, and stir and mix evenly;
[0028] 4) Add 2 parts of 1.2-benzisothiazolin-3 ketone and stir for 15 minutes;
[0029] 5) Add 2 parts of hardness polyethylene emulsion and stir for 5 minutes, filter and pack.
Embodiment 3
[0031] 1) Put in 25 parts of acrylic resin and 25 parts of water, start the machine to stir, and put in 45 parts of pigment during the stirring process;
[0032] 2) After stirring for 20 minutes, add 1 part of dispersant and 4 parts of defoamer, grind for 3 hours, and filter the material with a 2 μm filter.
[0033] 3) Add 48 parts of water-based acrylic emulsion, 22 parts of water, and 25 parts of color paste in sequence, and stir and mix evenly;
[0034] 4) Add 2 parts of 1.2-benzisothiazolin-3-one and stir for 15 minutes;
[0035] 5) Add 3 parts of hardness polyethylene emulsion and stir for 5 minutes, filter and pack.
[0036] The average molecular weight of the polypropylene resin used in the above examples is 400,000, the average molecular weight of the aqueous polypropylene emulsion is 200,000, the glass transition temperature is 20° C., and the hardness of the polyethylene emulsion is 5.
[0037] Compared with the original solvent-based ink, the product obtained by t...
PUM
Property | Measurement | Unit |
---|---|---|
glass transition temperature | aaaaa | aaaaa |
hardness | aaaaa | aaaaa |
hardness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com